General
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Density | 1.12 g/cm³ Show Supplier Material materials with Density of 1.12 g/cm³ | dry | ISO 1183 | |||
Moisture absorption | 23 °C | 2.1 % Show Supplier Material materials with Moisture absorption of 2.1 % | 50%RH | ISO 62 | 2 mm | |
Water absorption | 8.9 % Show Supplier Material materials with Water absorption of 8.9 % | ISO 62 | 2 mm | immersion at 23°C |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elastic modulus | 3.1 GPa Show Supplier Material materials with Elastic modulus of 3.1 GPa | dry | ISO 527-2/1A | 1mm/min | |
Elongation | 55 % Show Supplier Material materials with Elongation of 55 % | dry | ISO 527-2/1A | 50mm/min | nominal | |
Elongation at yield | 4.5 % Show Supplier Material materials with Elongation at yield of 4.5 % | dry | ISO 527-2/1A | 50mm/min | |
Flexural modulus | 3 GPa Show Supplier Material materials with Flexural modulus of 3 GPa | dry | ISO 178 | 2mm/min | |
Flexural strength | 115 MPa Show Supplier Material materials with Flexural strength of 115 MPa | dry | ISO 178 | 2mm/min | |
Impact strength, Charpy notched | 23 °C | 5.5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 5.5 kJ/m² | dry | ISO 179/1eA | |
Yield strength | 80 MPa Show Supplier Material materials with Yield strength of 80 MPa | dry | ISO 527-2/1A | 50mm/min |
Thermal
Property | Value | Testing Standard | Comment | ||
---|---|---|---|---|---|
Heat deflection temperature | 80 °C Show Supplier Material materials with Heat deflection temperature of 80 °C | ISO 75/2Af | 1.80 MPa | ||
Melting point | 260 °C Show Supplier Material materials with Melting point of 260 °C | ISO 11357-1/-3 | 10°C/min | ||
Vicat softening temperature | 240 °C Show Supplier Material materials with Vicat softening temperature of 240 °C | ISO 306 | 50°C/h 50N | ||
Flammability | Automotive Interior Flammability(mm/min): 0 ,method: ISO 3795 and thickness tested (mm): 3 |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Surface resistivity | 1e+10 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+10 Ω/sq | 50%RH | IEC 60093 | 500V |
1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | dry | IEC 60093 | 500V | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | 50%RH | IEC 60093 | 500V |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Shrinkage | 1.1 % Show Supplier Material materials with Shrinkage of 1.1 % | 290/60/60* | ISO 294-4 | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa] |
1.1 % Show Supplier Material materials with Shrinkage of 1.1 % | 290/60/60* | ISO 294-4 | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa], Transverse |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Natural brown | |
Features | Heat Stabilized | |
Processing methods | Injection Molding |