General
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Density | 1.46 g/cm³ Show Supplier Material materials with Density of 1.46 g/cm³ | dry | ISO 1183 | |||
Moisture absorption | 23 °C | 1.5 % Show Supplier Material materials with Moisture absorption of 1.5 % | 50%RH | ISO 62 | 2 mm | |
Water absorption | 5.5 % Show Supplier Material materials with Water absorption of 5.5 % | ISO 62 | 2 mm | immersion at 23°C |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elastic modulus | 8.5 GPa Show Supplier Material materials with Elastic modulus of 8.5 GPa | 50%RH | ISO 527-2/1A | 1mm/min | |
12.7 GPa Show Supplier Material materials with Elastic modulus of 12.7 GPa | dry | ISO 527-2/1A | 1mm/min | ||
Elongation | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-2/1A | 5mm/min | |
3.5 % Show Supplier Material materials with Elongation of 3.5 % | 50%RH | ISO 527-2/1A | 5mm/min | ||
Flexural modulus | 11.5 GPa Show Supplier Material materials with Flexural modulus of 11.5 GPa | dry | ISO 178 | 2mm/min | |
Flexural strength | 290 MPa Show Supplier Material materials with Flexural strength of 290 MPa | dry | ISO 178 | 2mm/min | |
Impact strength, Charpy notched | 23 °C | 15 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 15 kJ/m² | dry | ISO 179/1eA | |
23 °C | 20 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 20 kJ/m² | 50%RH | ISO 179/1eA | ||
Impact strength, Charpy unnotched | 95 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 95 kJ/m² | dry | ISO 179/1eU | 23°C | |
105 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 105 kJ/m² | 50%RH | ISO 179/1eU | 23°C | ||
Tensile strength | 120 MPa Show Supplier Material materials with Tensile strength of 120 MPa | 50%RH | ISO 527-2/1A | 5mm/min | |
190 MPa Show Supplier Material materials with Tensile strength of 190 MPa | dry | ISO 527-2/1A | 5mm/min |
Thermal
Property | Value | Testing Standard | Comment | ||
---|---|---|---|---|---|
Heat deflection temperature | 210 °C Show Supplier Material materials with Heat deflection temperature of 210 °C | ISO 75/2Af | 1.00E+12mm | ||
Melting point | 220 °C Show Supplier Material materials with Melting point of 220 °C | ISO 11357-1/-3 | 10°C/min | ||
Flammability | Thickness tested (mm): 0.8, Class: HB, Standard: UL 94 | Automotive Interior Flammability(mm/min): 0 ,method: ISO 3795 and thickness tested (mm): 3 |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Surface resistivity | 1e+10 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+10 Ω/sq | 50%RH | IEC 60093 | 500V |
1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | dry | IEC 60093 | 500V | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | 50%RH | IEC 60093 | 500V |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Features | Heat Stabilized | |
Fillers | 40% Glass Fiber | |
Processing methods | Injection Molding |