General
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Density | 1.06 g/cm³ Show Supplier Material materials with Density of 1.06 g/cm³ | dry | ISO 1183 | |||
Moisture absorption | 23 °C | 1.8 % Show Supplier Material materials with Moisture absorption of 1.8 % | 50%RH | ISO 62 | 2 mm | |
Water absorption | 7 % Show Supplier Material materials with Water absorption of 7 % | ISO 62 | 2 mm | immersion at 23°C |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elastic modulus | 0.5 GPa Show Supplier Material materials with Elastic modulus of 0.5 GPa | 50%RH | ISO 527-2/1A | 1mm/min | |
1.2 GPa Show Supplier Material materials with Elastic modulus of 1.2 GPa | dry | ISO 527-2/1A | 1mm/min | ||
Elongation | 100 % Show Supplier Material materials with Elongation of 100 % | dry, 50%RH | ISO 527-2/1A | min. | 50mm/min | nominal | |
Elongation at yield | 6.5 % Show Supplier Material materials with Elongation at yield of 6.5 % | dry | ISO 527-2/1A | 50mm/min | |
Flexural modulus | 0.4 GPa Show Supplier Material materials with Flexural modulus of 0.4 GPa | 50%RH | ISO 178 | 2mm/min | |
1.1 GPa Show Supplier Material materials with Flexural modulus of 1.1 GPa | dry | ISO 178 | 2mm/min | ||
Flexural strength | 18 MPa Show Supplier Material materials with Flexural strength of 18 MPa | 50%RH | ISO 178 | 2mm/min | |
45 MPa Show Supplier Material materials with Flexural strength of 45 MPa | dry | ISO 178 | 2mm/min | ||
Impact strength, Charpy notched | -30 °C | 30 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 30 kJ/m² | dry | ISO 179/1eA | |
23 °C | 70 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 70 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 90 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 90 kJ/m² | 50%RH | ISO 179/1eA | ||
Yield strength | 20 MPa Show Supplier Material materials with Yield strength of 20 MPa | 50%RH | ISO 527-2/1A | 50mm/min | |
34 MPa Show Supplier Material materials with Yield strength of 34 MPa | dry | ISO 527-2/1A | 50mm/min |
Thermal
Property | Value | Testing Standard | Thickness | Comment | |||
---|---|---|---|---|---|---|---|
Coefficient of thermal expansion | 0.00014 1/K Show Supplier Material materials with Coefficient of thermal expansion of 0.00014 1/K | ISO 11359-1/-2 | 23°C-55°C | ||||
0.00014 1/K Show Supplier Material materials with Coefficient of thermal expansion of 0.00014 1/K | ISO 11359-1/-2 | 23°C-55°C, Transverse | |||||
Glow Wire Flammability Index | 650 °C Show Supplier Material materials with Glow Wire Flammability Index of 650 °C | IEC 60695-2-12 | 2 mm | ||||
Glow Wire Ignition Temperature | 675 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 675 °C | IEC 60695-2-13 | 2 mm | ||||
Heat deflection temperature | 50 °C Show Supplier Material materials with Heat deflection temperature of 50 °C | ISO 75/2Af | 1.80 MPa | ||||
80 °C Show Supplier Material materials with Heat deflection temperature of 80 °C | ISO 75/2Bf | 0.45 MPa | |||||
Melting point | 220 °C Show Supplier Material materials with Melting point of 220 °C | ISO 11357-1/-3 | 10°C/min | ||||
Vicat softening temperature | 105 °C Show Supplier Material materials with Vicat softening temperature of 105 °C | ISO 306 | 50°C/h 50N | ||||
Flammability | Thickness tested (mm): 1.6, Class: HB, Standard: UL 94 | Automotive Interior Flammability(mm/min): <30 ,method: ISO 3795 and thickness tested (mm): 3 |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 500 V Show Supplier Material materials with Comparative tracking index of 500 V | dry | IEC 60112 | Sol.A |
Surface resistivity | 1e+10 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+10 Ω/sq | 50%RH | IEC 60093 | 500V |
1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | dry | IEC 60093 | 500V | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | 50%RH | IEC 60093 | 500V |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Features | Impact Modified | |
Processing methods | Injection Molding |