General
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Density | 1.37 g/cm³ Show Supplier Material materials with Density of 1.37 g/cm³ | dry | ISO 1183 | |||
Moisture absorption | 23 °C | 2 % Show Supplier Material materials with Moisture absorption of 2 % | 50%RH | ISO 62 | 2 mm | |
Water absorption | 7 % Show Supplier Material materials with Water absorption of 7 % | ISO 62 | 2 mm | immersion at 23°C |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elastic modulus | 5.4 GPa Show Supplier Material materials with Elastic modulus of 5.4 GPa | 50%RH | ISO 527-2/1A | 1mm/min | |
9.3 GPa Show Supplier Material materials with Elastic modulus of 9.3 GPa | dry | ISO 527-2/1A | 1mm/min | ||
Elongation | 2.6 % Show Supplier Material materials with Elongation of 2.6 % | dry | ISO 527-2/1A | 5mm/min | |
3.6 % Show Supplier Material materials with Elongation of 3.6 % | 50%RH | ISO 527-2/1A | 5mm/min | ||
Flexural modulus | 4.7 GPa Show Supplier Material materials with Flexural modulus of 4.7 GPa | 50%RH | ISO 178 | 2mm/min | |
8.4 GPa Show Supplier Material materials with Flexural modulus of 8.4 GPa | dry | ISO 178 | 2mm/min | ||
Flexural strength | 135 MPa Show Supplier Material materials with Flexural strength of 135 MPa | 50%RH | ISO 178 | 2mm/min | |
210 MPa Show Supplier Material materials with Flexural strength of 210 MPa | dry | ISO 178 | 2mm/min | ||
Impact strength, Charpy notched | 23 °C | 8 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 kJ/m² | dry | ISO 179/1eA | |
23 °C | 12 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 12 kJ/m² | 50%RH | ISO 179/1eA | ||
Impact strength, Charpy unnotched | 55 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 55 kJ/m² | dry | ISO 179/1eU | 23°C | |
70 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 70 kJ/m² | 50%RH | ISO 179/1eU | 23°C | ||
Tensile strength | 85 MPa Show Supplier Material materials with Tensile strength of 85 MPa | 50%RH | ISO 527-2/1A | 5mm/min | |
135 MPa Show Supplier Material materials with Tensile strength of 135 MPa | dry | ISO 527-2/1A | 5mm/min |
Thermal
Property | Value | Testing Standard | Comment | ||
---|---|---|---|---|---|
Heat deflection temperature | 190 °C Show Supplier Material materials with Heat deflection temperature of 190 °C | ISO 75/2Af | 1.80 MPa | ||
215 °C Show Supplier Material materials with Heat deflection temperature of 215 °C | ISO 75/2Bf | 0.45 MPa | |||
Melting point | 220 °C Show Supplier Material materials with Melting point of 220 °C | ISO 11357-1/-3 | 10°C/min | ||
Flammability | Thickness tested (mm): 0.8, Class: HB, Standard: UL 94 |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Surface resistivity | 1e+12 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+12 Ω/sq | dry | IEC 60093 | 500V |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Features | Heat Stabilized | |
Fillers | 30% Glass Fiber | |
Processing methods | Injection Molding |