General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.12 g/cm³ Show Supplier Material materials with Density of 1.12 g/cm³ | dry | ISO 1183 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elastic modulus | 0.85 GPa Show Supplier Material materials with Elastic modulus of 0.85 GPa | 50%RH | ISO 527-2/1A | 1mm/min | |
2.5 GPa Show Supplier Material materials with Elastic modulus of 2.5 GPa | dry | ISO 527-2/1A | 1mm/min | ||
Elongation | 20 % Show Supplier Material materials with Elongation of 20 % | dry | ISO 527-2/1A | min. | 50mm/min | nominal | |
Elongation at yield | 230 % Show Supplier Material materials with Elongation at yield of 230 % | 50%RH | ISO 527-2/1A | 50mm/min | |
Flexural modulus | 0.72 GPa Show Supplier Material materials with Flexural modulus of 0.72 GPa | 50%RH | ISO 178 | 2mm/min | |
2.5 GPa Show Supplier Material materials with Flexural modulus of 2.5 GPa | dry | ISO 178 | 2mm/min | ||
Flexural strength | 30 MPa Show Supplier Material materials with Flexural strength of 30 MPa | 50%RH | ISO 178 | 2mm/min | |
100 MPa Show Supplier Material materials with Flexural strength of 100 MPa | dry | ISO 178 | 2mm/min | ||
Impact strength, Charpy notched | 23 °C | 12.5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 12.5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 90 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 90 kJ/m² | 50%RH | ISO 179/1eA | ||
Impact strength, Charpy unnotched | No Break at 23°C | dry | ISO 179/1eU | ||
Yield strength | 35 MPa Show Supplier Material materials with Yield strength of 35 MPa | 50%RH | ISO 527-2/1A | 50mm/min | |
65 MPa Show Supplier Material materials with Yield strength of 65 MPa | dry | ISO 527-2/1A | 50mm/min |
Thermal
Rheological Properties
Property | Value | Testing Standard | Condition | Comment |
---|---|---|---|---|
Melt mass-flow rate | 20 g/10min Show Supplier Material materials with Melt mass-flow rate of 20 g/10min | ISO 1133 | 250°C/2.16Kg | |
Shrinkage | 1.4 % Show Supplier Material materials with Shrinkage of 1.4 % | ISO 294-4 | 250/80/60* | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa] |
1.6 % Show Supplier Material materials with Shrinkage of 1.6 % | ISO 294-4 | 250/80/60* | *Melt Temp. [°C] / Mold Temp. [°C] / Cavity Press. [MPa], Transverse |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Features | Impact Modified, Heat Stabilized | |
Processing methods | Injection Molding |