1.2190 (X37Cr13) Quenched and Tempered steel plate with corrosion resistant and very good polishability.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValueThickness

Thickness

255.0 mm

Show Supplier Material materials with Thickness of 255.0 mm

255.0 mm

355.0 mm

Show Supplier Material materials with Thickness of 355.0 mm

355.0 mm

Width

900 mm

Show Supplier Material materials with Width of 900 mm

Mechanical

PropertyValueComment

Hardness, Brinell

230.0

Show Supplier Material materials with Hardness, Brinell of 230.0

soft annealed

Hardness, Rockwell C

40.0 - 56.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 40.0 - 56.0 [-]

Tensile strength

1555.0 - 1775.0 MPa

Show Supplier Material materials with Tensile strength of 1555.0 - 1775.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000107 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000107 1/K

for 20°C to the mentioned temperature

150 °C

0.000011 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.000011 1/K

for 20°C to the mentioned temperature

200 °C

0.0000112 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000112 1/K

for 20°C to the mentioned temperature

250 °C

0.0000115 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000115 1/K

for 20°C to the mentioned temperature

300 °C

0.0000117 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000117 1/K

for 20°C to the mentioned temperature

350 °C

0.0000119 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000119 1/K

for 20°C to the mentioned temperature

400 °C

0.0000121 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000121 1/K

for 20°C to the mentioned temperature

450 °C

0.0000123 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000123 1/K

for 20°C to the mentioned temperature

500 °C

0.0000124 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000124 1/K

for 20°C to the mentioned temperature

Thermal conductivity

23 °C

21.5 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 21.5 W/(m·K)

150 °C

23.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 23.2 W/(m·K)

300 °C

23.9 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 23.9 W/(m·K)

350 °C

24.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24.3 W/(m·K)

400 °C

24.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24.2 W/(m·K)

500 °C

24 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24 W/(m·K)

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.37

Show Supplier Material materials with Carbon of 0.37

Chromium

13.6

Show Supplier Material materials with Chromium of 13.6

Manganese

0.5

Show Supplier Material materials with Manganese of 0.5

Silicon

0.9

Show Supplier Material materials with Silicon of 0.9

Vanadium

0.30000000000000004

Show Supplier Material materials with Vanadium of 0.30000000000000004

Technological properties

Property
Application areas

Moulds and inserts for processing corrosive acting plastics.

Heat Treatment

Soft annealing: 760-800°C (Cooling in furnace) - Hardening: 1000-1050°C and quenching in air, oil or hot bath T=500-550°C