1.2210 (115CrV3) Quenched and Tempered chromium-vanadium alloyoed cold-work steel bar that is wear resistant.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Diameter

5.0 mm

Show Supplier Material materials with Diameter of 5.0 mm

40.0 mm

Show Supplier Material materials with Diameter of 40.0 mm

Mechanical

PropertyValueComment

Hardness, Brinell

220.0

Show Supplier Material materials with Hardness, Brinell of 220.0

soft annealed

Hardness, Rockwell C

58.0 - 62.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 58.0 - 62.0 [-]

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.00001 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.00001 1/K

for 20°C to the mentioned temperature

200 °C

0.0000127 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000127 1/K

for 20°C to the mentioned temperature

300 °C

0.0000137 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000137 1/K

for 20°C to the mentioned temperature

400 °C

0.0000142 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000142 1/K

for 20°C to the mentioned temperature

500 °C

0.0000149 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000149 1/K

for 20°C to the mentioned temperature

600 °C

0.0000158 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000158 1/K

for 20°C to the mentioned temperature

700 °C

0.0000168 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000168 1/K

for 20°C to the mentioned temperature

Thermal conductivity

20 °C

34.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 34.2 W/(m·K)

350 °C

32.6 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 32.6 W/(m·K)

700 °C

31 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 31 W/(m·K)

Chemical properties

PropertyValue

Carbon

1.2

Show Supplier Material materials with Carbon of 1.2

Chromium

0.7000000000000001

Show Supplier Material materials with Chromium of 0.7000000000000001

Manganese

0.35000000000000003

Show Supplier Material materials with Manganese of 0.35000000000000003

Silicon

0.2

Show Supplier Material materials with Silicon of 0.2

Vanadium

0.1

Show Supplier Material materials with Vanadium of 0.1

Technological properties

Property
Application areas

Piercing dies, guide rods, twist drills, ejector pins and wood chisels

Heat Treatment

Soft annealing: 710-750°C (Cooling in furnace) - Stress-relief-annealing: 650-680°C, Hardening: 810-840°C (in oil) 780-810°C (in water)