Formadur 2316 Plate

Alternative and trade names
DIN EN ISO X38CrMo16, AISI 420mod, 1.2316,
Want to keep this datasheet? Save it now in your required format

Description

1.2316 (X38CrMo16) exhibits increased corrosion resistance and good polishability. Usually this steel grade is supplied in a quenched and tempered condition with a working hardness of approx. 300 HB.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValueThickness

Thickness

20.0 mm

Show Supplier Material materials with Thickness of 20.0 mm

20.0 mm

300.0 mm

Show Supplier Material materials with Thickness of 300.0 mm

300.0 mm

Width

700.0 mm

Show Supplier Material materials with Width of 700.0 mm

1150.0 mm

Show Supplier Material materials with Width of 1150.0 mm

Mechanical

PropertyValueComment

Hardness, Brinell

265.0 - 310.0 [-]

Show Supplier Material materials with Hardness, Brinell of 265.0 - 310.0 [-]

as-delivered condition

Hardness, Rockwell C

32.0 - 49.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 32.0 - 49.0 [-]

Tensile strength

900.0 - 1060.0 MPa

Show Supplier Material materials with Tensile strength of 900.0 - 1060.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000105 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000105 1/K

for 20°C to the mentioned temperature

150 °C

0.0000107 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000107 1/K

for 20°C to the mentioned temperature

200 °C

0.0000108 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000108 1/K

for 20°C to the mentioned temperature

250 °C

0.0000109 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000109 1/K

for 20°C to the mentioned temperature

300 °C

0.0000111 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000111 1/K

for 20°C to the mentioned temperature

350 °C

0.0000113 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000113 1/K

for 20°C to the mentioned temperature

400 °C

0.0000115 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000115 1/K

for 20°C to the mentioned temperature

450 °C

0.0000116 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000116 1/K

for 20°C to the mentioned temperature

500 °C

0.0000117 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000117 1/K

for 20°C to the mentioned temperature

Thermal conductivity

23 °C

23.5 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 23.5 W/(m·K)

150 °C

24.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24.2 W/(m·K)

300 °C

24.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24.3 W/(m·K)

350 °C

24.4 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24.4 W/(m·K)

400 °C

24.1 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24.1 W/(m·K)

500 °C

23.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 23.2 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.36

Show Supplier Material materials with Carbon of 0.36

Chromium

16.0

Show Supplier Material materials with Chromium of 16.0

Manganese

0.9

Show Supplier Material materials with Manganese of 0.9

Molybdenum

1.2

Show Supplier Material materials with Molybdenum of 1.2

Silicon

0.4

Show Supplier Material materials with Silicon of 0.4

Technological properties

Property
Application areas

Moulds for processing plastics with higher demands on corrosion resistance, tools for plastic extrusion.

Heat Treatment

Soft annealing: 760-800°C (Cooling in furnace) - Hardening: 1020-1050°C and quenching in oil or salt bath 500-520°C