Formadur PH X Superclean Plate

Alternative and trade names
X5CrNiCuNb15-5
Want to keep this datasheet? Save it now in your required format

Description

(X5CrNiCuNb15-5) Formadur PH X Superclean precipitation hardened steel has improved corrosion-resistance, high strength, excellent polishability due to the applied remelting process.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValueThickness

Thickness

200.0 mm

Show Supplier Material materials with Thickness of 200.0 mm

200.0 mm

500.0 mm

Show Supplier Material materials with Thickness of 500.0 mm

500.0 mm

Width

900.0 mm

Show Supplier Material materials with Width of 900.0 mm

1100.0 mm

Show Supplier Material materials with Width of 1100.0 mm

Mechanical

PropertyValue

Hardness, Rockwell C

38.0 - 42.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 38.0 - 42.0 [-]

Tensile strength

1190.0 - 1320.0 MPa

Show Supplier Material materials with Tensile strength of 1190.0 - 1320.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000104 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000104 1/K

for 20°C to the mentioned temperature

150 °C

0.0000106 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000106 1/K

for 20°C to the mentioned temperature

200 °C

0.0000109 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000109 1/K

for 20°C to the mentioned temperature

250 °C

0.0000111 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000111 1/K

for 20°C to the mentioned temperature

300 °C

0.0000114 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000114 1/K

for 20°C to the mentioned temperature

350 °C

0.0000115 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000115 1/K

for 20°C to the mentioned temperature

400 °C

0.0000117 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000117 1/K

for 20°C to the mentioned temperature

450 °C

0.0000119 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000119 1/K

for 20°C to the mentioned temperature

500 °C

0.000012 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.000012 1/K

for 20°C to the mentioned temperature

Thermal conductivity

23 °C

16.8 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 16.8 W/(m·K)

150 °C

20.1 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 20.1 W/(m·K)

300 °C

22.1 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 22.1 W/(m·K)

350 °C

22.8 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 22.8 W/(m·K)

400 °C

23.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 23.3 W/(m·K)

500 °C

24.1 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24.1 W/(m·K)

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.05

Show Supplier Material materials with Carbon of 0.05

Chromium

15.0

Show Supplier Material materials with Chromium of 15.0

Manganese

0.30000000000000004

Show Supplier Material materials with Manganese of 0.30000000000000004

Nickel

4.5

Show Supplier Material materials with Nickel of 4.5

Silicon

0.30000000000000004

Show Supplier Material materials with Silicon of 0.30000000000000004

Technological properties

Property
Application areas

High polished tools and moulds for processing of high corrosive plastics, tools for plastic extrusion.

Heat Treatment

Formadur PH X Superclean usually is supplied in precipitation-hardened condition with a hardness of 40 HRC.