Thermodur 2329 Bar

Alternative and trade names
DIN EN ISO 46CrSiMoV7, 1.2329
Want to keep this datasheet? Save it now in your required format

Description

46CrSiMoV7 (1.2329) shows the following features and properties:


  • Excellent tempering resistance
  • High-temperature strength
  • Full quenching and tempering properties
  • Outstanding weldability
  • Good machinability
  • Nitridable
  • PVD and CVD coatable
  • Equivalent Materials

    This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    Dimension

    PropertyValue

    Diameter

    232.0 mm

    Show Supplier Material materials with Diameter of 232.0 mm

    532.0 mm

    Show Supplier Material materials with Diameter of 532.0 mm

    Mechanical

    PropertyValueComment

    Hardness, Brinell

    230.0

    Show Supplier Material materials with Hardness, Brinell of 230.0

    soft annealed

    Hardness, Rockwell C

    46.0 - 52.0 [-]

    Show Supplier Material materials with Hardness, Rockwell C of 46.0 - 52.0 [-]

    Tensile strength

    1485.0 - 1775.0 MPa

    Show Supplier Material materials with Tensile strength of 1485.0 - 1775.0 MPa

    Chemical properties

    PropertyValue

    Carbon

    0.45

    Show Supplier Material materials with Carbon of 0.45

    Chromium

    1.8

    Show Supplier Material materials with Chromium of 1.8

    Manganese

    0.8

    Show Supplier Material materials with Manganese of 0.8

    Molybdenum

    0.30000000000000004

    Show Supplier Material materials with Molybdenum of 0.30000000000000004

    Nickel

    0.6000000000000001

    Show Supplier Material materials with Nickel of 0.6000000000000001

    Silicon

    0.7000000000000001

    Show Supplier Material materials with Silicon of 0.7000000000000001

    Vanadium

    0.2

    Show Supplier Material materials with Vanadium of 0.2

    Technological properties

    Property
    Application areas

    Forging dies, extrusion press tools, compression moulding dies

    Heat Treatment

    Soft annealing: 780-800°C (Cooling in furnace or air) - Hardening: 880-920°C and quenching in air, oil or hot bath T=500-550°C

    Welding

    Outstanding weldability