Thermodur 2714 Plate

Alternative and trade names
DIN EN ISO 55NiCrMoV7, 1.2714, AISI L6, AFNOR 55NCDV7
Want to keep this datasheet? Save it now in your required format

Description

1.2714 (55NiCrMoV7) is a tough die steel with high tempering resistance and good through-hardening properties. This grade is usually supplied in annealed condition or quenched and tempered to a working hardness of 370 to 410 HB (round) or 355 to 400 HB (square, flat).

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Dimensions

Thickness: 20.0 - 600.0 mm | Width: 350.0 - 1010.0 mm

Mechanical

PropertyValueComment

Hardness, Brinell

355 - 410 [-]

Show Supplier Material materials with Hardness, Brinell of 355 - 410 [-]

as-delivered condition

Hardness, Rockwell C

56 - 58 [-]

Show Supplier Material materials with Hardness, Rockwell C of 56 - 58 [-]

after quenching

Tensile strength

1190 - 1385 MPa

Show Supplier Material materials with Tensile strength of 1190 - 1385 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

1.22e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.22e-05 1/K

for 20°C to the mentioned temperature

200 °C

1.3e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.3e-05 1/K

for 20°C to the mentioned temperature

300 °C

1.33e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.33e-05 1/K

for 20°C to the mentioned temperature

400 °C

1.37e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.37e-05 1/K

for 20°C to the mentioned temperature

500 °C

1.42e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.42e-05 1/K

for 20°C to the mentioned temperature

600 °C

1.44e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.44e-05 1/K

for 20°C to the mentioned temperature

Thermal conductivity

23 °C

36 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 36 W/(m·K)

350 °C

38.8 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 38.8 W/(m·K)

700 °C

35 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 35 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.56 %

Show Supplier Material materials with Carbon of 0.56 %

Chromium

1.1 %

Show Supplier Material materials with Chromium of 1.1 %

Iron

Balance

Manganese

0.75 %

Show Supplier Material materials with Manganese of 0.75 %

Nickel

1.7 %

Show Supplier Material materials with Nickel of 1.7 %

Silicon

0.25 %

Show Supplier Material materials with Silicon of 0.25 %

Vanadium

0.1 %

Show Supplier Material materials with Vanadium of 0.1 %

Technological properties

Property
Application areas

Standard steel for forging dies, press dies, auxiliary tools for extrusion, die holders, armoured trim dies, hot shear blades

Heat Treatment

Soft annealing: 650-700°C (Cooling in furnace) - Hardening: 830-870°C, 860-900 (Oil, Air)