Description

1.2311 (40CrMnMo7) Tempered plastic mould steel, delivery hardness 280 to 325 HB. Good machinability, suitable for graining, better polishing properties than Formadur 2312.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Diameter

20.5 mm

Show Supplier Material materials with Diameter of 20.5 mm

151.5 mm

Show Supplier Material materials with Diameter of 151.5 mm

Mechanical

PropertyValueComment

Hardness, Brinell

280.0 - 325.0 [-]

Show Supplier Material materials with Hardness, Brinell of 280.0 - 325.0 [-]

as-delivered condition

Hardness, Rockwell C

28.0 - 51.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 28.0 - 51.0 [-]

Tensile strength

950.0 - 1095.0 MPa

Show Supplier Material materials with Tensile strength of 950.0 - 1095.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000126 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000126 1/K

for 20°C to the mentioned temperature

150 °C

0.0000128 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000128 1/K

for 20°C to the mentioned temperature

200 °C

0.000013 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.000013 1/K

for 20°C to the mentioned temperature

250 °C

0.0000133 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000133 1/K

for 20°C to the mentioned temperature

300 °C

0.0000135 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000135 1/K

for 20°C to the mentioned temperature

350 °C

0.0000137 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000137 1/K

for 20°C to the mentioned temperature

400 °C

0.0000139 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000139 1/K

for 20°C to the mentioned temperature

450 °C

0.0000141 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000141 1/K

for 20°C to the mentioned temperature

500 °C

0.0000143 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000143 1/K

for 20°C to the mentioned temperature

Thermal conductivity

23 °C

32.5 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 32.5 W/(m·K)

150 °C

32.9 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 32.9 W/(m·K)

300 °C

31.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 31.3 W/(m·K)

350 °C

30.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 30.2 W/(m·K)

400 °C

29.5 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 29.5 W/(m·K)

500 °C

27.4 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 27.4 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.4

Show Supplier Material materials with Carbon of 0.4

Chromium

1.9

Show Supplier Material materials with Chromium of 1.9

Manganese

1.5

Show Supplier Material materials with Manganese of 1.5

Molybdenum

0.2

Show Supplier Material materials with Molybdenum of 0.2

Silicon

0.30000000000000004

Show Supplier Material materials with Silicon of 0.30000000000000004

Technological properties

Property
Application areas

Plastic moulds, mould frames for plastic moulds and die casting moulds

Heat Treatment

Soft annealing: 710-740°C (Cooling in furnace) - Hardening: 840-870°C and quenching in oil or salt bath T=180-220°C