1.2343 (X37CrMoV5-1) is a hot-work alloy steel with extra fine structure (homogeneous grain structure) for homogeneous properties. It exhibits high hot tensile strength and toughness, good thermal conductivity and insusceptibility to hot cracking. It can be water-cooled to a limited extent.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValueThickness

Thickness

30.0 mm

Show Supplier Material materials with Thickness of 30.0 mm

30.0 mm

500.0 mm

Show Supplier Material materials with Thickness of 500.0 mm

500.0 mm

Width

610.0 mm

Show Supplier Material materials with Width of 610.0 mm

1010.0 mm

Show Supplier Material materials with Width of 1010.0 mm

Mechanical

PropertyValueComment

Hardness, Brinell

230.0

Show Supplier Material materials with Hardness, Brinell of 230.0

annealed

Hardness, Rockwell C

42.0 - 52.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 42.0 - 52.0 [-]

Tensile strength

1320.0 - 1775.0 MPa

Show Supplier Material materials with Tensile strength of 1320.0 - 1775.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000118 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000118 1/K

for 20°C to the mentioned temperature

200 °C

0.0000124 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000124 1/K

for 20°C to the mentioned temperature

300 °C

0.0000126 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000126 1/K

for 20°C to the mentioned temperature

400 °C

0.0000127 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000127 1/K

for 20°C to the mentioned temperature

500 °C

0.0000128 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000128 1/K

for 20°C to the mentioned temperature

600 °C

0.0000129 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000129 1/K

for 20°C to the mentioned temperature

700 °C

0.0000129 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000129 1/K

for 20°C to the mentioned temperature

Thermal conductivity

20 °C

26.8 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 26.8 W/(m·K)

350 °C

27.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 27.3 W/(m·K)

700 °C

30.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 30.3 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.38

Show Supplier Material materials with Carbon of 0.38

Chromium

5.3

Show Supplier Material materials with Chromium of 5.3

Manganese

0.4

Show Supplier Material materials with Manganese of 0.4

Silicon

1.0

Show Supplier Material materials with Silicon of 1.0

Vanadium

0.4

Show Supplier Material materials with Vanadium of 0.4

Technological properties

Property
Application areas

Universally usable e.g. casting dies and moulds for light metal processing, mandrel bars, forging dies and inserts, shrink rings, hot shear blades, ejector pins and tools for plastic processing

Heat Treatment