Thermodur 2365 EFS Bar

Alternative and trade names
DIN EN ISO 32CrMoV12-28, 1.2365, AISI H10, AFNOR 32CDV12-28
Want to keep this datasheet? Save it now in your required format

Description

1.2365 (32CrMoV12-28) is a steel bar with excellent high-temperature strength and tempering resistance, thermal conductivity, low susceptibility to hot cracking. May be water-cooled to a limited extent. Suitable for cold hobbing.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Diameter

25.8 mm

Show Supplier Material materials with Diameter of 25.8 mm

353.0 mm

Show Supplier Material materials with Diameter of 353.0 mm

Mechanical

PropertyValueComment

Hardness, Brinell

185.0

Show Supplier Material materials with Hardness, Brinell of 185.0

soft annealed

Hardness, Rockwell C

40.0 - 50.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 40.0 - 50.0 [-]

Tensile strength

1255.0 - 1665.0 MPa

Show Supplier Material materials with Tensile strength of 1255.0 - 1665.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000118 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000118 1/K

for 20°C to the mentioned temperature

200 °C

0.0000125 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000125 1/K

for 20°C to the mentioned temperature

300 °C

0.0000127 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000127 1/K

for 20°C to the mentioned temperature

400 °C

0.0000131 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000131 1/K

for 20°C to the mentioned temperature

500 °C

0.0000135 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000135 1/K

for 20°C to the mentioned temperature

600 °C

0.0000136 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000136 1/K

for 20°C to the mentioned temperature

700 °C

0.0000138 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000138 1/K

for 20°C to the mentioned temperature

Thermal conductivity

20 °C

31.4 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 31.4 W/(m·K)

350 °C

32 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 32 W/(m·K)

700 °C

29.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 29.3 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.32

Show Supplier Material materials with Carbon of 0.32

Chromium

3.0

Show Supplier Material materials with Chromium of 3.0

Manganese

0.30000000000000004

Show Supplier Material materials with Manganese of 0.30000000000000004

Silicon

0.25

Show Supplier Material materials with Silicon of 0.25

Vanadium

0.5

Show Supplier Material materials with Vanadium of 0.5

Technological properties

Property
Application areas

High speed forging machines, dies and inserts, extrusion dies for steel and heavy metal processing, heavy metal die casting tools, piercer plugs, steel for high alternating thermal stress

Heat Treatment

Soft annealing: 750-800°C (Cooling in furnace) - Hardening: 1030-1050°C and quenching in air, oil or hot bath T=500-550°C