Thermodur 2999 EFS Superclean Bar

Want to keep this datasheet? Save it now in your required format

Description

1.2999 (X45MoCrV5-3-1) is a Quenched and Tempered steel bar that shows the following features and properties:


  • Exhibits maximum high-temperature strength
  • Good high-temperature wear resistance
  • Excellent thermal shock resistance
  • Excellent thermal conductivity across the entire range of service temperatures
  • Equivalent Materials

    This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    Dimension

    PropertyValue

    Diameter

    25.8 mm

    Show Supplier Material materials with Diameter of 25.8 mm

    252.0 mm

    Show Supplier Material materials with Diameter of 252.0 mm

    Mechanical

    PropertyValueComment

    Hardness, Brinell

    230.0

    Show Supplier Material materials with Hardness, Brinell of 230.0

    soft annealed

    Hardness, Rockwell C

    42.0 - 52.0 [-]

    Show Supplier Material materials with Hardness, Rockwell C of 42.0 - 52.0 [-]

    Tensile strength

    1320.0 - 1775.0 MPa

    Show Supplier Material materials with Tensile strength of 1320.0 - 1775.0 MPa

    Thermal

    PropertyTemperatureValueComment

    Coefficient of thermal expansion

    100 °C

    0.0000113 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000113 1/K

    for 20°C to the mentioned temperature

    200 °C

    0.0000119 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000119 1/K

    for 20°C to the mentioned temperature

    300 °C

    0.0000122 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000122 1/K

    for 20°C to the mentioned temperature

    400 °C

    0.0000126 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000126 1/K

    for 20°C to the mentioned temperature

    500 °C

    0.000013 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000013 1/K

    for 20°C to the mentioned temperature

    600 °C

    0.0000133 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000133 1/K

    for 20°C to the mentioned temperature

    700 °C

    0.0000135 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000135 1/K

    for 20°C to the mentioned temperature

    Thermal conductivity

    20 °C

    31.4 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 31.4 W/(m·K)

    350 °C

    35.2 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 35.2 W/(m·K)

    700 °C

    36.2 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 36.2 W/(m·K)

    Chemical properties

    PropertyValue

    Carbon

    0.45

    Show Supplier Material materials with Carbon of 0.45

    Chromium

    3.0

    Show Supplier Material materials with Chromium of 3.0

    Manganese

    0.30000000000000004

    Show Supplier Material materials with Manganese of 0.30000000000000004

    Silicon

    0.30000000000000004

    Show Supplier Material materials with Silicon of 0.30000000000000004

    Vanadium

    1.0

    Show Supplier Material materials with Vanadium of 1.0

    Technological properties

    Property
    Application areas

    For use at highest temperatures, highly wear-exposed die inserts, high speed forging machines, casting dies for heavy metal processing

    Heat Treatment

    Soft annealing: 750-800°C (Cooling in furnace) - Hardening: 1070-1100°C and quenching in air, oil or hot bath T=500-550°C