Dimension
Property | Value |
---|---|
Thickness | 150 - 400 mm Show Supplier Material materials with Thickness of 150 - 400 mm |
Width | 850 mm Show Supplier Material materials with Width of 850 mm |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Hardness, Brinell | 230 [-] Show Supplier Material materials with Hardness, Brinell of 230 [-] at 23.0 °C | 23.0 °C | soft annealed |
Hardness, Rockwell C | 42 - 52 [-] Show Supplier Material materials with Hardness, Rockwell C of 42 - 52 [-] at 23.0 °C | 23.0 °C | |
Tensile strength | 1320 - 1775 MPa Show Supplier Material materials with Tensile strength of 1320 - 1775 MPa at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 1.15E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.15E-5 1/K at 100.0 °C | 100.0 °C | for 20°C to the mentioned temperature |
1.2E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.2E-5 1/K at 200.0 °C | 200.0 °C | for 20°C to the mentioned temperature | |
1.23E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.23E-5 1/K at 300.0 °C | 300.0 °C | for 20°C to the mentioned temperature | |
1.26E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.26E-5 1/K at 400.0 °C | 400.0 °C | for 20°C to the mentioned temperature | |
1.29E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.29E-5 1/K at 500.0 °C | 500.0 °C | for 20°C to the mentioned temperature | |
1.32E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.32E-5 1/K at 600.0 °C | 600.0 °C | for 20°C to the mentioned temperature | |
Thermal conductivity | 28.36 W/(m·K) Show Supplier Material materials with Thermal conductivity of 28.36 W/(m·K) at 20.0 °C | 20.0 °C | |
29.3 W/(m·K) Show Supplier Material materials with Thermal conductivity of 29.3 W/(m·K) at 100.0 °C | 100.0 °C | ||
30.9 W/(m·K) Show Supplier Material materials with Thermal conductivity of 30.9 W/(m·K) at 200.0 °C | 200.0 °C | ||
31 W/(m·K) Show Supplier Material materials with Thermal conductivity of 31 W/(m·K) at 300.0 °C | 300.0 °C | ||
30.7 W/(m·K) Show Supplier Material materials with Thermal conductivity of 30.7 W/(m·K) at 400.0 °C | 400.0 °C | ||
29.5 W/(m·K) Show Supplier Material materials with Thermal conductivity of 29.5 W/(m·K) at 500.0 °C | 500.0 °C | ||
27.8 W/(m·K) Show Supplier Material materials with Thermal conductivity of 27.8 W/(m·K) at 600.0 °C | 600.0 °C | ||
Chemical properties
Property | ||
---|---|---|
Carbon | 0.35 % | |
Chromium | 5 % | |
Iron | Balance | |
Manganese | 0.3 % | |
Other | Plus additions | |
Silicon | 0.3 % | |
Vanadium | 0.8 % |
Technological properties
Property | ||
---|---|---|
Application areas | Universally usable for highly stressed tools and highest temperatures, casting dies for light metal processing (especially for complex tools), extrusion dies for light and heavy metal processing (especially for complexly formed profiles), dies and inserts | |
Heat Treatment | Soft annealing: 750-800°C (Cooling in furnace) - Hardening: 1020-1040°C and quenching in air, oil or hot bath T=500-550°C |