Cryodur 2357

Alternative and trade names
DIN EN ISO 50CrMoV13-14, 1.2357,AISI S7
Want to keep this datasheet? Save it now in your required format

Description

1.2357 (50CrMoV13-15) Quenched and Tempered steel bar that shows the following features and properties:


  • High toughness
  • High wear resistance
  • High compression strength
  • Dimensional stability
  • Good polishability
  • Equivalent Materials

    This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    Mechanical

    PropertyValueComment

    Hardness, Brinell

    220.0

    Show Supplier Material materials with Hardness, Brinell of 220.0

    soft annealed

    Hardness, Rockwell C

    54.0 - 58.0 [-]

    Show Supplier Material materials with Hardness, Rockwell C of 54.0 - 58.0 [-]

    Tensile strength

    1665.0 - 2180.0 MPa

    Show Supplier Material materials with Tensile strength of 1665.0 - 2180.0 MPa

    Thermal

    PropertyTemperatureValueComment

    Coefficient of thermal expansion

    200 °C

    0.0000122 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000122 1/K

    for 20°C to the mentioned temperature

    400 °C

    0.0000125 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000125 1/K

    for 20°C to the mentioned temperature

    Thermal conductivity

    100 °C

    28.9 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 28.9 W/(m·K)

    200 °C

    30 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 30 W/(m·K)

    400 °C

    31 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 31 W/(m·K)

    Chemical properties

    PropertyValue

    Carbon

    0.5

    Show Supplier Material materials with Carbon of 0.5

    Chromium

    3.35

    Show Supplier Material materials with Chromium of 3.35

    Manganese

    0.7000000000000001

    Show Supplier Material materials with Manganese of 0.7000000000000001

    Molybdenum

    1.6

    Show Supplier Material materials with Molybdenum of 1.6

    Silicon

    0.30000000000000004

    Show Supplier Material materials with Silicon of 0.30000000000000004

    Vanadium

    0.25

    Show Supplier Material materials with Vanadium of 0.25

    Technological properties

    Property
    Application areas

    Punching tools, moulds, scrap shears, piercing dies, hobs, coining dies, plastic moulds, tableting tools

    Heat Treatment

    Soft annealing: 610-650°C (Cooling in furnace) - Stress-relief-annealing: 600°C, Hardening: 920-970°C and quenching in oil or air