Cryodur 2379 Bar

Alternative and trade names
DIN EN ISO X153CrMoV12, 1.2379,AISI D2,AFNOR Z160CDV12
Want to keep this datasheet? Save it now in your required format

Description

1.2379 (X153CrMoV12) 12% Ledeburitic Quenched and Tempered Chromium steel bar that shows the following features and properties:


  • Maximum wear resistance
  • Good toughness
  • Outstanding cutting edge retention
  • Outstanding tempering resistance
  • Nitridable after special heat treatment
  • Equivalent Materials

    This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    Dimension

    PropertyValue

    Diameter

    20.5 mm

    Show Supplier Material materials with Diameter of 20.5 mm

    758.0 mm

    Show Supplier Material materials with Diameter of 758.0 mm

    Mechanical

    PropertyValueComment

    Hardness, Brinell

    250.0

    Show Supplier Material materials with Hardness, Brinell of 250.0

    soft annealed

    Hardness, Rockwell C

    56.0 - 62.0 [-]

    Show Supplier Material materials with Hardness, Rockwell C of 56.0 - 62.0 [-]

    Thermal

    PropertyTemperatureValueComment

    Coefficient of thermal expansion

    100 °C

    0.0000105 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000105 1/K

    for 20°C to the mentioned temperature

    200 °C

    0.0000115 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000115 1/K

    for 20°C to the mentioned temperature

    300 °C

    0.0000119 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000119 1/K

    for 20°C to the mentioned temperature

    400 °C

    0.0000122 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.0000122 1/K

    for 20°C to the mentioned temperature

    Thermal conductivity

    20 °C

    16.7 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 16.7 W/(m·K)

    350 °C

    20.5 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 20.5 W/(m·K)

    700 °C

    24.2 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 24.2 W/(m·K)

    Chemical properties

    PropertyValue

    Carbon

    1.55

    Show Supplier Material materials with Carbon of 1.55

    Chromium

    12.0

    Show Supplier Material materials with Chromium of 12.0

    Manganese

    0.35000000000000003

    Show Supplier Material materials with Manganese of 0.35000000000000003

    Molybdenum

    0.75

    Show Supplier Material materials with Molybdenum of 0.75

    Silicon

    0.30000000000000004

    Show Supplier Material materials with Silicon of 0.30000000000000004

    Vanadium

    0.9

    Show Supplier Material materials with Vanadium of 0.9

    Technological properties

    Property
    Application areas

    Threading rolls and dies, cold extrusion tools, trimming, cutting and stamping tools, precision cutting tools, cold pilger mandrels, rotary shear blades, deep-drawing tools, highly wear-resistant plastic moulds

    Heat Treatment

    Soft annealing: 830-860°C (Cooling in furnace) - Stress-relief-annealing: 650-700°C (cooling in Furnace), Hardening: 1000-1050°C and quenching in oil, air or salt bath: 500-550°C