Cryodur 2436 Bar

Alternative and trade names
DIN EN ISO X210CrW12, 1.2436,AISI D6,AFNOR Z210CW12-01
Want to keep this datasheet? Save it now in your required format

Description

1.2436 (X210CrW12) 12% Ledeburitic Quenched and Tempered Chromium steel bar with very high wear resistance and cutting edge retention as well as improved hardenability.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Diameter

81.0 mm

Show Supplier Material materials with Diameter of 81.0 mm

403.0 mm

Show Supplier Material materials with Diameter of 403.0 mm

Mechanical

PropertyValueComment

Hardness, Brinell

250.0

Show Supplier Material materials with Hardness, Brinell of 250.0

soft annealed

Hardness, Rockwell C

58.0 - 62.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 58.0 - 62.0 [-]

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000109 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000109 1/K

for 20°C to the mentioned temperature

200 °C

0.0000119 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000119 1/K

for 20°C to the mentioned temperature

300 °C

0.0000123 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000123 1/K

for 20°C to the mentioned temperature

400 °C

0.0000126 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000126 1/K

for 20°C to the mentioned temperature

500 °C

0.0000129 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000129 1/K

for 20°C to the mentioned temperature

600 °C

0.000013 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.000013 1/K

for 20°C to the mentioned temperature

700 °C

0.0000132 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000132 1/K

for 20°C to the mentioned temperature

Thermal conductivity

20 °C

16.7 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 16.7 W/(m·K)

350 °C

20.5 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 20.5 W/(m·K)

700 °C

24.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 24.2 W/(m·K)

Chemical properties

PropertyValue

Carbon

2.1

Show Supplier Material materials with Carbon of 2.1

Chromium

12.0

Show Supplier Material materials with Chromium of 12.0

Manganese

0.35000000000000003

Show Supplier Material materials with Manganese of 0.35000000000000003

Silicon

0.35000000000000003

Show Supplier Material materials with Silicon of 0.35000000000000003

Tungsten

0.7000000000000001

Show Supplier Material materials with Tungsten of 0.7000000000000001

Technological properties

Property
Application areas

Blanking dies for cutting transformer and dynamo sheets, paper and plastics, deep-drawing tools, drawing dies and mandrels, shear blades

Heat Treatment

Soft annealing: 800-840°C (Cooling in furnace) - Stress-relief-annealing: 650-700°C (cooling in Furnace), Hardening: 950-980°C and quenching in oil, air or salt bath: 500-550°C