Cryodur 2510 Bar

Alternative and trade names
DIN EN ISO 100MnCrW4, 1.2510,AISI O1,AFNOR 90MWCV5
Want to keep this datasheet? Save it now in your required format

Description

1.2510 (100MnCrW4) Quenched and Tempered steel bar that shows good cutting edge retention and high hardenability & dimensional stability during heat treatment.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Diameter

12.0 mm

Show Supplier Material materials with Diameter of 12.0 mm

302.0 mm

Show Supplier Material materials with Diameter of 302.0 mm

Mechanical

PropertyValueComment

Hardness, Brinell

230.0

Show Supplier Material materials with Hardness, Brinell of 230.0

soft annealed

Hardness, Rockwell C

54.0 - 61.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 54.0 - 61.0 [-]

Thermal

PropertyTemperatureValue

Thermal conductivity

20 °C

33.5 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 33.5 W/(m·K)

350 °C

32 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 32 W/(m·K)

700 °C

30.9 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 30.9 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.9500000000000001

Show Supplier Material materials with Carbon of 0.9500000000000001

Chromium

0.6000000000000001

Show Supplier Material materials with Chromium of 0.6000000000000001

Manganese

1.1

Show Supplier Material materials with Manganese of 1.1

Silicon

0.2

Show Supplier Material materials with Silicon of 0.2

Tungsten

0.6000000000000001

Show Supplier Material materials with Tungsten of 0.6000000000000001

Vanadium

0.1

Show Supplier Material materials with Vanadium of 0.1

Technological properties

Property
Application areas

Blanking and stamping dies for cutting sheets, threading tools, drills, broaches, gauges, measuring tools, plastic moulds, shear blades, guide rails

Heat Treatment

Soft annealing: 800-840°C (Cooling in furnace) - Stress-relief-annealing: 650-700°C (cooling in Furnace), Hardening: 950-980°C and quenching in oil, air or salt bath: 500-550°C