Cryodur 2550 Bar

Alternative and trade names
DIN EN ISO 60WCrV8, 1.2550,AISI S1,AFNOR 55WC20
Want to keep this datasheet? Save it now in your required format

Description

1.2550 (60WCrV8) Quenched and Tempered cold work tool steel bar with impact-resistance that characterized by very good toughness in combination with high hardenability.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Diameter

20.5 mm

Show Supplier Material materials with Diameter of 20.5 mm

121.5 mm

Show Supplier Material materials with Diameter of 121.5 mm

Mechanical

PropertyValueComment

Hardness, Brinell

225.0

Show Supplier Material materials with Hardness, Brinell of 225.0

soft annealed

Hardness, Rockwell C

54.0 - 58.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 54.0 - 58.0 [-]

Tensile strength

1920.0 - 2180.0 MPa

Show Supplier Material materials with Tensile strength of 1920.0 - 2180.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000118 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000118 1/K

for 20°C to the mentioned temperature

200 °C

0.0000127 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000127 1/K

for 20°C to the mentioned temperature

300 °C

0.0000131 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000131 1/K

for 20°C to the mentioned temperature

400 °C

0.0000135 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000135 1/K

for 20°C to the mentioned temperature

500 °C

0.000014 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.000014 1/K

for 20°C to the mentioned temperature

600 °C

0.0000143 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000143 1/K

for 20°C to the mentioned temperature

700 °C

0.0000145 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000145 1/K

for 20°C to the mentioned temperature

Thermal conductivity

20 °C

34.2 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 34.2 W/(m·K)

350 °C

32.6 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 32.6 W/(m·K)

700 °C

30.9 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 30.9 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.6000000000000001

Show Supplier Material materials with Carbon of 0.6000000000000001

Chromium

1.1

Show Supplier Material materials with Chromium of 1.1

Manganese

0.35000000000000003

Show Supplier Material materials with Manganese of 0.35000000000000003

Silicon

0.6000000000000001

Show Supplier Material materials with Silicon of 0.6000000000000001

Tungsten

2.0

Show Supplier Material materials with Tungsten of 2.0

Vanadium

0.2

Show Supplier Material materials with Vanadium of 0.2

Technological properties

Property
Application areas

Blanking dies for cutting sheets, trimming and splitting dies, cold piercing punches, tableting tools, shear blades, chopping knives, pneumatic chisels, coining tools, cold shear blades, ejectors

Heat Treatment

Soft annealing: 710-750°C (Cooling in furnace) - Stress-relief-annealing: 650°C (cooling in Furnace), Hardening: 870-900°C and quenching in oil or salt bath: 500-550°C