Tempered mould steel with improved quenching and tempering properties, good machinability, polishable, weldable and can be textured. This grade offers substantial improvements, especially for building larger and complex moulds. Specific modifications of the grade's components as well as additional smelting and secondary metallurgy ensure Formadur® 320's outstanding properties. We recommend the use of Formadur® 320 Superclean (ESR) for the highest demands.

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Mechanical

PropertyValueComment

Hardness, Brinell

280 - 385 [-]

Show Supplier Material materials with Hardness, Brinell of 280 - 385 [-]

as-delivered condition

Hardness, Rockwell C

28 - 51 [-]

Show Supplier Material materials with Hardness, Rockwell C of 28 - 51 [-]

Tensile strength

1060 - 1190 MPa

Show Supplier Material materials with Tensile strength of 1060 - 1190 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

1.11e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.11e-05 1/K

for 20°C to the mentioned temperature

200 °C

1.29e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.29e-05 1/K

for 20°C to the mentioned temperature

300 °C

1.34e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.34e-05 1/K

for 20°C to the mentioned temperature

400 °C

1.35e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.35e-05 1/K

for 20°C to the mentioned temperature

500 °C

1.38e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.38e-05 1/K

for 20°C to the mentioned temperature

600 °C

1.41e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.41e-05 1/K

for 20°C to the mentioned temperature

700 °C

1.43e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.43e-05 1/K

for 20°C to the mentioned temperature

Thermal conductivity

23 °C

36 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 36 W/(m·K)

150 °C

37.4 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 37.4 W/(m·K)

300 °C

33 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 33 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.34 %

Show Supplier Material materials with Carbon of 0.34 %

Chromium

1.7 %

Show Supplier Material materials with Chromium of 1.7 %

Iron

Balance

Manganese

0.8 %

Show Supplier Material materials with Manganese of 0.8 %

Molybdenum

0.4 %

Show Supplier Material materials with Molybdenum of 0.4 %

Nickel

0.5 %

Show Supplier Material materials with Nickel of 0.5 %

Silicon

0.4 %

Show Supplier Material materials with Silicon of 0.4 %

Technological properties

Property
Application areas

As Formadur 320 with highest demands on polishability

Heat Treatment

Soft annealing: 710-740°C (Cooling in furnace) - Hardening: 820-850°C and quenching in oil or polymer