Cryodur 2767 Plate

Alternative and trade names
DIN EN ISO 45NiCrMo16, 1.2767, AISI 6F3
Want to keep this datasheet? Save it now in your required format

Description

1.2767 (45NiCrMo16) Quenched and Tempered steel plate with high hardenability and toughness, highly suitable for polishing, texturing and EDM machining. We recommend the use of Cryodur 2767 (ESR) for exttreme demands.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Thickness

25 - 350 mm

Show Supplier Material materials with Thickness of 25 - 350 mm

Width

1010 mm

Show Supplier Material materials with Width of 1010 mm

Mechanical

PropertyValueComment

Hardness, Brinell

260 [-]

Show Supplier Material materials with Hardness, Brinell of 260 [-]

soft annealed

Hardness, Rockwell C

48 - 54 [-]

Show Supplier Material materials with Hardness, Rockwell C of 48 - 54 [-]

Tensile strength

1555 - 1920 MPa

Show Supplier Material materials with Tensile strength of 1555 - 1920 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

1.2e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.2e-05 1/K

for 20°C to the mentioned temperature | Quenched and Tempered

200 °C

1.25e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.25e-05 1/K

for 20°C to the mentioned temperature | Quenched and Tempered

300 °C

1.3e-05 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 1.3e-05 1/K

for 20°C to the mentioned temperature | Quenched and Tempered

Thermal conductivity

100 °C

27.7 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 27.7 W/(m·K)

150 °C

28.9 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 28.9 W/(m·K)

200 °C

29.7 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 29.7 W/(m·K)

250 °C

30.5 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 30.5 W/(m·K)

300 °C

31 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 31 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.45 %

Show Supplier Material materials with Carbon of 0.45 %

Chromium

1.4 %

Show Supplier Material materials with Chromium of 1.4 %

Iron

Balance

Manganese

0.35 %

Show Supplier Material materials with Manganese of 0.35 %

Molybdenum

0.2 %

Show Supplier Material materials with Molybdenum of 0.2 %

Nickel

4 %

Show Supplier Material materials with Nickel of 4 %

Silicon

0.25 %

Show Supplier Material materials with Silicon of 0.25 %

Technological properties

Property
Application areas

Cutlery dies, cutting tools for thick materials, billet-shear blades, drawing jaws, massive embossing and bending tools, plastic moulds, reinforcements

Heat Treatment

Soft annealing: 610-650°C (Cooling in furnace) - Stress-relief-annealing: 600-650°C (cooling in Furnace), Hardening: 840-870°C and quenching in air, oil or salt bath: 180-220°C