Dimension
Property | Value |
---|---|
Thickness | 15 - 200 mm Show Supplier Material materials with Thickness of 15 - 200 mm |
Width | 1010 mm Show Supplier Material materials with Width of 1010 mm |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Hardness, Brinell | 220 [-] Show Supplier Material materials with Hardness, Brinell of 220 [-] at 23.0 °C | 23.0 °C | soft annealed |
Hardness, Rockwell C | 56 - 60 [-] Show Supplier Material materials with Hardness, Rockwell C of 56 - 60 [-] at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 1.22E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.22E-5 1/K at 100.0 °C | 100.0 °C | for 20°C to the mentioned temperature |
1.32E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.32E-5 1/K at 200.0 °C | 200.0 °C | for 20°C to the mentioned temperature | |
1.38E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.38E-5 1/K at 300.0 °C | 300.0 °C | for 20°C to the mentioned temperature | |
1.43E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.43E-5 1/K at 400.0 °C | 400.0 °C | for 20°C to the mentioned temperature | |
1.47E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.47E-5 1/K at 500.0 °C | 500.0 °C | for 20°C to the mentioned temperature | |
1.5E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.5E-5 1/K at 600.0 °C | 600.0 °C | for 20°C to the mentioned temperature | |
1.53E-5 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.53E-5 1/K at 700.0 °C | 700.0 °C | for 20°C to the mentioned temperature | |
Thermal conductivity | 33 W/(m·K) Show Supplier Material materials with Thermal conductivity of 33 W/(m·K) at 20.0 °C | 20.0 °C | |
32 W/(m·K) Show Supplier Material materials with Thermal conductivity of 32 W/(m·K) at 350.0 °C | 350.0 °C | ||
32.3 W/(m·K) Show Supplier Material materials with Thermal conductivity of 32.3 W/(m·K) at 700.0 °C | 700.0 °C | ||
Chemical properties
Property | ||
---|---|---|
Carbon | 0.9 % | |
Chromium | 0.4 % | |
Iron | Balance | |
Manganese | 2 % | |
Silicon | 0.2 % | |
Vanadium | 0.1 % |
Technological properties
Property | ||
---|---|---|
Application areas | Universally usable, cutting and stamping tools, thread-cutting tools, reamers, gauges, measuring tools, plastic moulds, shear blades, guide rails, ejector pins | |
Heat Treatment | Soft annealing: 680-720°C (Cooling in furnace) - Stress-relief-annealing: 650°C (cooling in Furnace), Hardening: 790-820°C and quenching in air, oil or salt bath: 180-220°C |