Description

1.2842 (90MnCrV8) Quenched and Tempered steel bar with good cutting edge retention, dimensionally stable during heat treatment.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Dimension

PropertyValue

Diameter

20.5 mm

Show Supplier Material materials with Diameter of 20.5 mm

523.0 mm

Show Supplier Material materials with Diameter of 523.0 mm

Mechanical

PropertyValueComment

Hardness, Brinell

220.0

Show Supplier Material materials with Hardness, Brinell of 220.0

soft annealed

Hardness, Rockwell C

56.0 - 60.0 [-]

Show Supplier Material materials with Hardness, Rockwell C of 56.0 - 60.0 [-]

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000122 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000122 1/K

for 20°C to the mentioned temperature

200 °C

0.0000132 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000132 1/K

for 20°C to the mentioned temperature

300 °C

0.0000138 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000138 1/K

for 20°C to the mentioned temperature

400 °C

0.0000143 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000143 1/K

for 20°C to the mentioned temperature

500 °C

0.0000147 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000147 1/K

for 20°C to the mentioned temperature

600 °C

0.000015 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.000015 1/K

for 20°C to the mentioned temperature

700 °C

0.0000153 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000153 1/K

for 20°C to the mentioned temperature

Thermal conductivity

20 °C

33 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 33 W/(m·K)

350 °C

32 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 32 W/(m·K)

700 °C

32.3 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 32.3 W/(m·K)

Chemical properties

PropertyValue

Carbon

0.9

Show Supplier Material materials with Carbon of 0.9

Chromium

0.4

Show Supplier Material materials with Chromium of 0.4

Manganese

2.0

Show Supplier Material materials with Manganese of 2.0

Silicon

0.2

Show Supplier Material materials with Silicon of 0.2

Vanadium

0.1

Show Supplier Material materials with Vanadium of 0.1

Technological properties

Property
Application areas

Universally usable, cutting and stamping tools, thread-cutting tools, reamers, gauges, measuring tools, plastic moulds, shear blades, guide rails, ejector pins

Heat Treatment

Soft annealing: 680-720°C (Cooling in furnace) - Stress-relief-annealing: 650°C (cooling in Furnace), Hardening: 790-820°C and quenching in air, oil or salt bath: 180-220°C