Cryodur 2990 Bar

Alternative and trade names
DIN EN ISO X100CrMoV8-1-1, 1.2290
Want to keep this datasheet? Save it now in your required format

Description

1.2290 (X100CrMoV8-1-1) Quenched and Tempered cold work tool steel bar that shows the following features and properties:


  • High compressive strength
  • High resistance to abrasive and adhesive wear
  • Good EDM properties
  • Good surface treatability by all known methods
  • Good inductive hardenability
  • Equivalent Materials

    This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    Properties

    Dimension

    PropertyValue

    Diameter

    25.8 mm

    Show Supplier Material materials with Diameter of 25.8 mm

    453.0 mm

    Show Supplier Material materials with Diameter of 453.0 mm

    Mechanical

    PropertyValueComment

    Hardness, Brinell

    250.0

    Show Supplier Material materials with Hardness, Brinell of 250.0

    soft annealed

    Hardness, Rockwell C

    57.0 - 63.0 [-]

    Show Supplier Material materials with Hardness, Rockwell C of 57.0 - 63.0 [-]

    Thermal

    PropertyTemperatureValueComment

    Coefficient of thermal expansion

    100 °C

    0.000114 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000114 1/K

    for 20°C to the mentioned temperature

    150 °C

    0.000116 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000116 1/K

    for 20°C to the mentioned temperature

    200 °C

    0.000117 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000117 1/K

    for 20°C to the mentioned temperature

    250 °C

    0.000119 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000119 1/K

    for 20°C to the mentioned temperature

    300 °C

    0.00012 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.00012 1/K

    for 20°C to the mentioned temperature

    350 °C

    0.000121 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000121 1/K

    for 20°C to the mentioned temperature

    400 °C

    0.000123 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000123 1/K

    for 20°C to the mentioned temperature

    450 °C

    0.000124 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000124 1/K

    for 20°C to the mentioned temperature

    500 °C

    0.000126 1/K

    Show Supplier Material materials with Coefficient of thermal expansion of 0.000126 1/K

    for 20°C to the mentioned temperature

    Thermal conductivity

    20 °C

    24 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 24 W/(m·K)

    100 °C

    25.9 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 25.9 W/(m·K)

    150 °C

    26.8 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 26.8 W/(m·K)

    200 °C

    27.1 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 27.1 W/(m·K)

    300 °C

    27.4 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 27.4 W/(m·K)

    400 °C

    27.52 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 27.52 W/(m·K)

    500 °C

    26.8 W/(m·K)

    Show Supplier Material materials with Thermal conductivity of 26.8 W/(m·K)

    Chemical properties

    PropertyValue

    Carbon

    1.0

    Show Supplier Material materials with Carbon of 1.0

    Chromium

    8.0

    Show Supplier Material materials with Chromium of 8.0

    Manganese

    0.35000000000000003

    Show Supplier Material materials with Manganese of 0.35000000000000003

    Molybdenum

    1.1

    Show Supplier Material materials with Molybdenum of 1.1

    Silicon

    0.9

    Show Supplier Material materials with Silicon of 0.9

    Vanadium

    1.6

    Show Supplier Material materials with Vanadium of 1.6

    Technological properties

    Property
    Application areas

    Cutting and punching tools including precision cutting tools, threading dies and rolls, rotary shear blades, cold pilger mandrels, strike plates, plastic moulds, coldforming and deep-drawing dies, woodworking tools, cold rolls

    Heat Treatment

    Soft annealing: 830-860°C (Cooling in furnace) - Stress-relief-annealing: 650°C (cooling in Furnace), Hardening: 1030-1080°C and quenching in air, oil or salt bath: 500-550°C