Acidur 4571 +AT

Alternative and trade names
Acidur 4571, 1.4571, Type 316Ti, SUS316Ti, X6CrNiMoTi17-12-2
Want to keep this datasheet? Save it now in your required format

Description

Acidur 4571 is comparable to Acidur 4404 in terms of corrosion resistance and mechanical and technological values, while Acidur 4057 is the material of choice if high strength at high temperatures is required. Due to the low carbon content, Acidur 4571 can also be used without heat treatment after welding.

Related Standards

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

8.0 g/cm³

Show Supplier Material materials with Density of 8.0 g/cm³

Dimension

PropertyValueComment

Diameter

250 mm

Show Supplier Material materials with Diameter of 250 mm

max.

Mechanical

PropertyTemperatureValue

Charpy impact energy, V-notch

100.0 J

Show Supplier Material materials with Charpy impact energy, V-notch of 100.0 J

Elastic modulus

20 °C

200 GPa

Show Supplier Material materials with Elastic modulus of 200 GPa

100 °C

194 GPa

Show Supplier Material materials with Elastic modulus of 194 GPa

200 °C

186 GPa

Show Supplier Material materials with Elastic modulus of 186 GPa

300 °C

179 GPa

Show Supplier Material materials with Elastic modulus of 179 GPa

400 °C

172 GPa

Show Supplier Material materials with Elastic modulus of 172 GPa

500 °C

165 GPa

Show Supplier Material materials with Elastic modulus of 165 GPa

Hardness, Brinell

215.0

Show Supplier Material materials with Hardness, Brinell of 215.0

Hardness, Rockwell C

22.0

Show Supplier Material materials with Hardness, Rockwell C of 22.0

Tensile strength

500.0 - 700.0 MPa

Show Supplier Material materials with Tensile strength of 500.0 - 700.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000165 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000165 1/K

for 20°C to the mentioned temperature

200 °C

0.0000175 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000175 1/K

for 20°C to the mentioned temperature

300 °C

0.000018 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.000018 1/K

for 20°C to the mentioned temperature

400 °C

0.0000185 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000185 1/K

for 20°C to the mentioned temperature

500 °C

0.000019 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.000019 1/K

for 20°C to the mentioned temperature

Unlock all property charts

Specific heat capacity

500.0 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 500.0 J/(kg·K)

Thermal conductivity

15 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 15 W/(m·K)

Electrical

PropertyValue

Electrical resistivity

7.5e-07 Ω·m

Show Supplier Material materials with Electrical resistivity of 7.5e-07 Ω·m

Chemical properties

PropertyValueComment

Carbon

0.08

Show Supplier Material materials with Carbon of 0.08

Chromium

16.5 - 18.5 %

Show Supplier Material materials with Chromium of 16.5 - 18.5 %

Manganese

2.0

Show Supplier Material materials with Manganese of 2.0

Molybdenum

2.0 - 2.5 %

Show Supplier Material materials with Molybdenum of 2.0 - 2.5 %

Nickel

10.5 - 13.5 %

Show Supplier Material materials with Nickel of 10.5 - 13.5 %

Phosphorus

0.045

Show Supplier Material materials with Phosphorus of 0.045

Silicon

1.0

Show Supplier Material materials with Silicon of 1.0

Sulfur

0.03

Show Supplier Material materials with Sulfur of 0.03

Titanium

0.7000000000000001

Show Supplier Material materials with Titanium of 0.7000000000000001

min: 5xC

Technological properties

Property
Application areas

Apparatus and pipeline construction, Construction industry, Chemical industry, Food industry, Mechanical Engineering, Medical and pharmaceutical industry, Shipbuilding

Corrosion properties

Acidur 4571 shows good corrosion resistance in most natural waters with low to medium concentrations of chlorides, salt and hydrochloric acid as well as organic acids. Since Acidur 4571 is resistant to intergranular corrosion even after welding, it meets the following standardized test methods: AFNOR NF 05-159, ASTM A262 Practice E and DIN EN ISO 3651 Part 2. (PREN = 23.1 – 26.7)

General machinability

The addition of titanium leads to the formation of titanium carbonitrides, which increases the tool wear

Heat Treatment

Solution annealing: 1020-1120°C (water, air) fast cooling

Hot forming

It is formable at 900-1200°C

Processing history

Solution Annealed

Welding

Acidur 4571 can be welded with and without filler material using all conventional methods. If a filler metal is necessary, use 1.4430. No heat treatment is required after welding. The interpass temperature should not exceed 200°C. Approach colours must be mechanically or chemically be removed.