Carbodur 6587 Blank Hardened

Alternative and trade names
Carbodur 6587, 1.6587, 18CrNiMo7-6
Want to keep this datasheet? Save it now in your required format

Description

1.6587 (18CrNiMo7-6) Blank Hardened Nickel Chromium Molybdenum Steel with good toughness and good machinability.

Equivalent Materials

This material data has been provided by Deutsche Edelstahlwerke Specialty Steel (DEW).

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

7.8 g/cm³

Show Supplier Material materials with Density of 7.8 g/cm³

Dimension

PropertyValueComment

Diameter

63 mm

Show Supplier Material materials with Diameter of 63 mm

max.

Mechanical

PropertyValueComment

Charpy impact energy, V-notch

41.0 J

Show Supplier Material materials with Charpy impact energy, V-notch of 41.0 J

Elastic modulus

210 GPa

Show Supplier Material materials with Elastic modulus of 210 GPa

Hardness, Brinell

179.0 - 229.0 [-]

Show Supplier Material materials with Hardness, Brinell of 179.0 - 229.0 [-]

Depending on the delivery condition

Reduction of area

30.0 - 35.0 %

Show Supplier Material materials with Reduction of area of 30.0 - 35.0 %

Tensile strength

980.0 - 1420.0 MPa

Show Supplier Material materials with Tensile strength of 980.0 - 1420.0 MPa

Yield strength

685.0 - 835.0 MPa

Show Supplier Material materials with Yield strength of 685.0 - 835.0 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100 °C

0.0000115 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000115 1/K

for 20°C to the mentioned temperature

200 °C

0.0000125 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000125 1/K

for 20°C to the mentioned temperature

300 °C

0.0000133 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000133 1/K

for 20°C to the mentioned temperature

400 °C

0.0000139 1/K

Show Supplier Material materials with Coefficient of thermal expansion of 0.0000139 1/K

for 20°C to the mentioned temperature

Specific heat capacity

431.0 J/(kg·K)

Show Supplier Material materials with Specific heat capacity of 431.0 J/(kg·K)

Thermal conductivity

39.8 W/(m·K)

Show Supplier Material materials with Thermal conductivity of 39.8 W/(m·K)

Electrical

PropertyValue

Electrical resistivity

1.2e-07 Ω·m

Show Supplier Material materials with Electrical resistivity of 1.2e-07 Ω·m

Chemical properties

PropertyValue

Carbon

0.15 - 0.21 %

Show Supplier Material materials with Carbon of 0.15 - 0.21 %

Chromium

1.5 - 1.8 %

Show Supplier Material materials with Chromium of 1.5 - 1.8 %

Manganese

0.5 - 0.9 %

Show Supplier Material materials with Manganese of 0.5 - 0.9 %

Molybdenum

0.25 - 0.35000000000000003 %

Show Supplier Material materials with Molybdenum of 0.25 - 0.35000000000000003 %

Nickel

1.4 - 1.7000000000000002 %

Show Supplier Material materials with Nickel of 1.4 - 1.7000000000000002 %

Phosphorus

0.025

Show Supplier Material materials with Phosphorus of 0.025

Silicon

0.4

Show Supplier Material materials with Silicon of 0.4

Sulfur

0.035

Show Supplier Material materials with Sulfur of 0.035

Technological properties

Property
Application areas

This steel is used for gearbox parts such as ring gears or drive pinion.

Heat Treatment

Soft annealing: 650-700°C (Oil, Polymer), Carburizing: 880-980°C (Oil, Polymer), Core Hardening 830-870°C (Oil, Polymer), Surface hardening: 780-820°C(Oil, Polymer), Tempering: 150-200°C (Air)

Hot forming

It is formable at 850-1100°C

Processing history

Blank Hardened

Welding

It is usually weldable.