3M™ Dyneon™ TFM™ (Modified PTFE Granules TFM 1705)

Want to keep this datasheet? Save it now in your required format

Description

Modified non-free-flowing suspension PTFE of the 2nd generation for compression moulding applications like diaphragms, shaped parts and skived films.


Special Features are:

  • Meets ASTM D 4894 Type III, Grade 1 classification
  • Produced by suspension polymerisation
  • Improved particle coalescence
  • Dense polymer structure with reduced void content
  • Low permeability
  • Substantially lower deformation under load (“cold flow”)
  • Very good electrical and mechanical properties
  • Improved gel stability
  • Increased modulus of elasticity
  • Good weldability
  • Improved flex life characteristics
  • Excellent chemical inertness
  • Low friction behaviour
  • Good flame retardance
  • Exceptional temperature resistance

  • Typical Properties:

    PTFE moulding powder with very small particle size is preferred for moulded parts requiring very good mechanical and electrical properties, a denser polymer structure, improved gel stability and flex life characteristics.

    This material data has been provided by Matmatch.

    All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
    Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

    Ashby charts

    See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

    Properties

    General

    PropertyTemperatureValueComment

    Bulk density

    23.0 °C

    0.41 g/cm³

    Show Material materials with Bulk density of 0.41 g/cm³

    DIN EN ISO 60

    Density

    23.0 °C

    2.16 g/cm³

    Show Material materials with Density of 2.16 g/cm³

    DIN EN ISO 12086

    Particle size

    25000 nm

    Show Material materials with Particle size of 25000 nm

    ISO 13320, average value

    Mechanical

    PropertyTemperatureValueComment

    Elastic modulus

    23.0 °C

    0.65 GPa

    Show Material materials with Elastic modulus of 0.65 GPa

    DIN EN ISO 527

    Elongation

    23.0 °C

    560 %

    Show Material materials with Elongation of 560 %

    DIN EN ISO 527-3, 0.1 mm film

    Hardness, Shore D

    23.0 °C

    59 [-]

    Show Material materials with Hardness, Shore D of 59 [-]

    DIN EN ISO 868

    Tensile strength

    23.0 °C

    47 MPa

    Show Material materials with Tensile strength of 47 MPa

    DIN EN ISO 527-3, 0.1 mm film

    Thermal

    PropertyTemperatureValueComment

    Coefficient of thermal expansion

    100.0 °C

    1.2E-4 1/K

    Show Material materials with Coefficient of thermal expansion of 1.2E-4 1/K

    DIN 53 752, from 30°C to the mentioned temperature

    200.0 °C

    1.4E-4 1/K

    Show Material materials with Coefficient of thermal expansion of 1.4E-4 1/K

    DIN 53 752, from 30°C to the mentioned temperature

    260.0 °C

    1.7E-4 1/K

    Show Material materials with Coefficient of thermal expansion of 1.7E-4 1/K

    DIN 53 752, from 30°C to the mentioned temperature

    Thermal conductivity

    23.0 °C

    0.22 W/(m·K)

    Show Material materials with Thermal conductivity of 0.22 W/(m·K)

    DIN 52612

    Flammability

    V-0 UL94

    Electrical

    PropertyTemperatureValueComment

    Dielectric strength

    23.0 °C

    90 kV/mm

    Show Material materials with Dielectric strength of 90 kV/mm

    DIN EN ISO 12086, 0.1 mm film

    Electrical resistivity

    23.0 °C

    1.00E+16 Ω·m

    Show Material materials with Electrical resistivity of 1.00E+16 Ω·m

    IEC 60093

    Surface resistivity

    23.0 °C

    1.00E+17 Ω/sq

    Show Material materials with Surface resistivity of 1.00E+17 Ω/sq

    IEC 60093

    Rheological Properties

    PropertyTemperatureValueComment

    Shrinkage

    23.0 °C

    5.4 %

    Show Material materials with Shrinkage of 5.4 %

    Internal Dyneon method, Cylinder 45 mm diameter

    Technological properties

    Property
    Application areas

    3MTM DyneonTM TFMTM Modified PTFE Powder TFM 1705 is a non-free-flowing compression moulding powder for applications like shaped parts, large walled cylinders or blocks with reduced elephant foot, skived films of > 20 μm, linings in the chemical processing industry (CPI) and especially valve and pump diaphragms with improved flex life.