Description

Unreinforced, opaque, provides chemical resistance and dimensional stability, UL94V-0 rated at 0.031".

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.33 g/cm³

Show Material materials with Density of 1.33 g/cm³

ASTM D 792

Water absorption

23.0 °C

0.14 %

Show Material materials with Water absorption of 0.14 %

ASTM D 570 | 24 Hours

Water absorption, equilibrium

23.0 °C

0.6 %

Show Material materials with Water absorption, equilibrium of 0.6 %

ASTM D 570

Mechanical

PropertyTemperatureValueComment

Elongation

23.0 °C

120 %

Show Material materials with Elongation of 120 %

ASTM D 638 | Type I, 50 mm/min

Flexural modulus

23.0 °C

2.24 GPa

Show Material materials with Flexural modulus of 2.24 GPa

ASTM D 790 | 1.3 mm/min, 50 mm span

Flexural strength

23.0 °C

68 MPa

Show Material materials with Flexural strength of 68 MPa

ASTM D 790 | 1.3 mm/min, 50 mm span

Flexural yield strength

23.0 °C

68 MPa

Show Material materials with Flexural yield strength of 68 MPa

ASTM D 790 | 1.3 mm/min, 50 mm span

Hardness, Rockwell R

23.0 °C

115 [-]

Show Material materials with Hardness, Rockwell R of 115 [-]

ASTM D 785

Impact strength, Izod notched, ASTM

-40.0 °C

170 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 170 J/m

ASTM D 256

-30.0 °C

192 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 192 J/m

ASTM D 256

23.0 °C

640 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 640 J/m

ASTM D 256

Tensile strength

23.0 °C

41 MPa

Show Material materials with Tensile strength of 41 MPa

ASTM D 638 | Type I, 50 mm/min

Yield strength

23.0 °C

41 MPa

Show Material materials with Yield strength of 41 MPa

ASTM D 638 | Type I, 50 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

8.28E-5 1/K

Show Material materials with Coefficient of thermal expansion of 8.28E-5 1/K

ASTM E 831 | 60°C to 138°C

Heat deflection temperature, 1.80 MPa

121 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 121 °C

ASTM D 648 | 1.82 MPa, 6.4 mm, unannealed

Relative temperature index, electrical

105 °C

Show Material materials with Relative temperature index, electrical of 105 °C

UL 746B

Relative temperature index, mechanical impact

105 °C

Show Material materials with Relative temperature index, mechanical impact of 105 °C

UL 746B

Relative temperature index, mechanical strength

105 °C

Show Material materials with Relative temperature index, mechanical strength of 105 °C

UL 746B

Flammability

UL Recognized, 94-5VA Flame Class Rating | 2.2mm | UL 94

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

3 V

Show Material materials with Comparative tracking index of 3 V

UL 746A

Dielectric constant

23.0 °C

5.7 [-]

Show Material materials with Dielectric constant of 5.7 [-]

ASTM D 150 | at 1 MHz

Dielectric strength

23.0 °C

12 kV/mm

Show Material materials with Dielectric strength of 12 kV/mm

ASTM D 149 | in oil, 3.2 mm

Dissipation factor

23.0 °C

0.03 [-]

Show Material materials with Dissipation factor of 0.03 [-]

ASTM D 150 | at 1 MHz

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

1 - 1.4 %

Show Material materials with Shrinkage of 1 - 1.4 %

SABIC method | 2.3-4.6 mm

Shrinkage, transverse

23.0 °C

1.2 - 1.6 %

Show Material materials with Shrinkage, transverse of 1.2 - 1.6 %

SABIC method | 2.3-4.6 mm

Technological properties

Property
Application areas

Circuit Protection,Electronic Components,Enclosure/Housing/Cover,Enclosures,Energy Management,Heavy Vehicles,Medical Device,Personal Computing,Surgical Devices,Wireless Communications

Processing methods

Drying Temperature: 120°C, Drying Time: 3-4hrs, Drying Time (Cumulative): 12hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 250-265°C, Nozzle Temperature: 245-260°C, Front - Zone 3 Temperature: 250-265°C, Middle - Zone 2 Temperature: 245-260°C, Rear - Zone 1 Temperature: 240-255°C, Mold Temperature: 50-75°C, Back Pressure: 0.3-0.7MPa, Screw Speed: 50-100rpm, Shot to Cylinder Size: 40-80%, Vent Depth: 0.025-0.038mm