CYCOLOY C6600 Polycarbonate/Acrylonitrile Butadiene Styrene (PC/ABS) blend is an injection moldable non chlorinated/brominated flame retardant grade with balanced flow, impact and hydrolytic stability. It also offers good chemical resistance and colorability in opaque colors. It has a UL94 V0@1.5mm and 5VB@2.0mm flame rating.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.19 g/cm³

Show Material materials with Density of 1.19 g/cm³

ISO 1183

Water absorption

23.0 °C

0.2 %

Show Material materials with Water absorption of 0.2 %

ISO 62 | 23°C, 50% RH

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.7 GPa

Show Material materials with Elastic modulus of 2.7 GPa

ISO 527 | 1 mm/min

Elongation at yield

23.0 °C

4 %

Show Material materials with Elongation at yield of 4 %

ISO 527 | 50 mm/min

Flexural modulus

23.0 °C

2.7 GPa

Show Material materials with Flexural modulus of 2.7 GPa

ISO 178 | 2 mm/min

Flexural yield strength

23.0 °C

90 MPa

Show Material materials with Flexural yield strength of 90 MPa

ISO 178 | 2 mm/min

Hardness, Ball Indentation

23.0 °C

110 MPa

Show Material materials with Hardness, Ball Indentation of 110 MPa

ISO 2039-1

Hardness, Rockwell R

23.0 °C

122 [-]

Show Material materials with Hardness, Rockwell R of 122 [-]

ISO 2039-2

Impact strength, Charpy notched

-30.0 °C

10 kJ/m²

Show Material materials with Impact strength, Charpy notched of 10 kJ/m²

ISO 179/1eA

23.0 °C

15 kJ/m²

Show Material materials with Impact strength, Charpy notched of 15 kJ/m²

ISO 179/1eA

Impact strength, Izod notched

-30.0 °C

10 kJ/m²

Show Material materials with Impact strength, Izod notched of 10 kJ/m²

ISO 180/1A

23.0 °C

15 kJ/m²

Show Material materials with Impact strength, Izod notched of 15 kJ/m²

ISO 180/1A

Unlock all property charts

Tensile strength

23.0 °C

50 MPa

Show Material materials with Tensile strength of 50 MPa

ISO 527 | 50 mm/min

Yield strength

23.0 °C

60 MPa

Show Material materials with Yield strength of 60 MPa

ISO 527 | 50 mm/min

Impact strength, Charpy unnotched

No Break @ 23,-30°C | ISO 179/1eU

Impact strength, Izod unnotched

No Break @ 23,-30°C| ISO 180/1U

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

8E-5 1/K

Show Material materials with Coefficient of thermal expansion of 8E-5 1/K

ISO 11359-2 | 23°C to 60°C

Coefficient of thermal expansion, transverse

23.0 °C

8E-5 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 8E-5 1/K

ISO 11359-2 | 23°C to 60°C

Heat deflection temperature, 1.80 MPa

80 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 80 °C

ISO 75/Ae | 1.8 MPa

Relative temperature index, electrical

80 °C

Show Material materials with Relative temperature index, electrical of 80 °C

UL 746B

Relative temperature index, mechanical impact

70 °C

Show Material materials with Relative temperature index, mechanical impact of 70 °C

UL 746B

Relative temperature index, mechanical strength

80 °C

Show Material materials with Relative temperature index, mechanical strength of 80 °C

UL 746B

Thermal conductivity

23.0 °C

0.2 W/(m·K)

Show Material materials with Thermal conductivity of 0.2 W/(m·K)

ISO 8302

Vicat softening temperature

107 °C

Show Material materials with Vicat softening temperature of 107 °C

ISO 306 | Rate B/120

Flammability

UL Recognized, 94-5VB Flame Class Rating | 2mm | UL 94

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

2 V

Show Material materials with Comparative tracking index of 2 V

UL 746A

Dielectric constant

23.0 °C

2.7 [-]

Show Material materials with Dielectric constant of 2.7 [-]

IEC 60250 | at 50/60 Hz

Dielectric strength

23.0 °C

17 kV/mm

Show Material materials with Dielectric strength of 17 kV/mm

IEC 60243-1 | in oil, 3.2 mm

Dissipation factor

23.0 °C

6E-3 [-]

Show Material materials with Dissipation factor of 6E-3 [-]

IEC 60250 | at 1 MHz

Rheological Properties

PropertyTemperatureValueComment

Melt volume-flow rate

16 cm³/10min

Show Material materials with Melt volume-flow rate of 16 cm³/10min

ISO 1133 | 260°C/2.16 kg

Shrinkage

23.0 °C

0.4 - 0.6 %

Show Material materials with Shrinkage of 0.4 - 0.6 %

SABIC method

Technological properties

Property
Application areas

Air Cabin Interiors,Air Conditioning,Air Filtration,Amusement Machine,Animal Testing,ATM/Ticket Machine,Audio,Auto Aftermarket,Building Accessory,Building Element,Circuit Protection,Coffee Maker/Espresso Machine,Commercial Storage/Cookware,Data Management,Data Transfer,Defense Vehicles,Dishwasher,Displays,Document Handling,Doors Hardware/Trim,Electronic Components,Enclosure/Housing/Cover,Enclosures,Energy Management,EV Infrastructure,Fluid Delivery,Food Processor,Food Transportation,Forward Lighting,Freezer,Gas/Electric Oven,Heavy Vehicles,Industrial Material Handling,Lab Ware and Clinical Diagnostics,Laundry Dryer,Lawn/Garden,LED Lighting,Medical Device,Medical Facility Infrastructure,Meter Gas,Microwave Oven,Modular Panel,Monitoring and Imaging,Non-LED Lighting,Personal Care,Personal Computing,Pharmaceutical Packaging & Drug Delivery,Photo/Video Camera,Photovoltaic Components,Plumbing,Power Manangement,Recreational Vehicle,Refrigerator,Renal and Blood Handling,Respiratory,Security/Detection,Small Appliance,Surgical Devices,Surgical Tray,Vacuum Cleaner,Vending Machine,Washing Machine,Watch/Jewelry,Water Treatment/Filtration,Wearables,Window,Wireless Communications,Wiring Devices,Wire & cable

Processing methods

Drying Temperature: 80-90°C, Drying Time: 2-4hrs, Melt Temperature: 250-270°C, Nozzle Temperature: 250-270°C, Front - Zone 3 Temperature: 250-270°C, Middle - Zone 2 Temperature: 240-260°C, Rear - Zone 1 Temperature: 230-250°C, Hopper Temperature: 60-80°C, Mold Temperature: 70-85°C