CYCOLOY™ FR Resins CY5025

Want to keep this datasheet? Save it now in your required format

Description

CYCOLOY CY5025 Polycarbonate/Acrylonitrile Butadiene Styrene (PC/ABS) resin is a standard grade that can be injection molded. This non-chlorinated, non-brominated flame retardant PC/ABS has a UL V0 & 5VB flame rating. CYCOLOY CY5025 resin is a general purpose resin that is an excellent candidate for a wide variety of thin wall applications.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.2 g/cm³

Show Material materials with Density of 1.2 g/cm³

ASTM D 792

Water absorption

23.0 °C

0.29 %

Show Material materials with Water absorption of 0.29 %

ISO 62

Mechanical

PropertyTemperatureValueComment

Elongation

23.0 °C

99 %

Show Material materials with Elongation of 99 %

ASTM D 638 | Type I, 50 mm/min

Flexural modulus

23.0 °C

2.88 GPa

Show Material materials with Flexural modulus of 2.88 GPa

ISO 178 | 2 mm/min

Flexural yield strength

23.0 °C

96 MPa

Show Material materials with Flexural yield strength of 96 MPa

ISO 178 | 2 mm/min

Impact strength, Charpy notched

23.0 °C

11 kJ/m²

Show Material materials with Impact strength, Charpy notched of 11 kJ/m²

ISO 179/1eA

Impact strength, Izod notched, ASTM

23.0 °C

450 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 450 J/m

ASTM D 256

Yield strength

23.0 °C

56 MPa

Show Material materials with Yield strength of 56 MPa

ASTM D 638 | Type I, 50 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 7E-5 1/K

ASTM E 831 | -40°C to 40°C

Coefficient of thermal expansion, transverse

23.0 °C

6.7E-5 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 6.7E-5 1/K

ASTM E 831 | -40°C to 40°C

Heat deflection temperature, 0.45 MPa

83 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 83 °C

ISO 75/Bf | 0.45 MPa

Relative temperature index, electrical

60 °C

Show Material materials with Relative temperature index, electrical of 60 °C

UL 746B

Relative temperature index, mechanical impact

60 °C

Show Material materials with Relative temperature index, mechanical impact of 60 °C

UL 746B

Relative temperature index, mechanical strength

60 °C

Show Material materials with Relative temperature index, mechanical strength of 60 °C

UL 746B

Flammability

UL Compliant, 94-5VB Rating | 1.5mm | UL 94 by SABIC-IP

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

0 V

Show Material materials with Comparative tracking index of 0 V

UL 746A

Volume resistivity

23.0 °C

1.00E+17 Ω·cm

Show Material materials with Volume resistivity of 1.00E+17 Ω·cm

ASTM D 257

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

27 g/10min

Show Material materials with Melt mass-flow rate of 27 g/10min

ASTM D 1238 | 260°C/2.16 kgf

Shrinkage

23.0 °C

0.23 %

Show Material materials with Shrinkage of 0.23 %

SABIC method | 1.5-3.2 mm

Shrinkage, transverse

23.0 °C

0.31 %

Show Material materials with Shrinkage, transverse of 0.31 %

SABIC method | 1.5-3.2 mm

Technological properties

Property
Application areas

Displays,Document Handling

Processing methods

Drying Temperature: 80-90°C, Drying Time: 3-4hrs, Drying Time (Cumulative): 8hrs, Maximum Moisture Content: 0.04%, Melt Temperature: 245-275°C, Nozzle Temperature: 245-275°C, Front - Zone 3 Temperature: 245-275°C, Middle - Zone 2 Temperature: 220-265°C, Rear - Zone 1 Temperature: 220-255°C, Mold Temperature: 60-80°C, Back Pressure: 0.3-0.7MPa, Screw Speed: 40-70rpm, Shot to Cylinder Size: 30-80%, Vent Depth: 0.038-0.076mm