LEXAN™ Resin LUX2180T

Want to keep this datasheet? Save it now in your required format

Description

Global grade. LEXAN LUX2180T is an injection moulding grade especially designed for manufacturing optical parts requiring easy flow properties combined with very high transmission and color stability. UV stabilized

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.2 g/cm³

Show Material materials with Density of 1.2 g/cm³

ISO 1183

Water absorption

23.0 °C

0.15 %

Show Material materials with Water absorption of 0.15 %

ISO 62 | 23°C, 50% RH

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.3 GPa

Show Material materials with Elastic modulus of 2.3 GPa

ISO 527 | 1 mm/min

Elongation

23.0 °C

100 %

Show Material materials with Elongation of 100 %

ISO 527 | 50 mm/min

Elongation at yield

23.0 °C

6 %

Show Material materials with Elongation at yield of 6 %

ISO 527 | 50 mm/min

Flexural modulus

23.0 °C

2.3 GPa

Show Material materials with Flexural modulus of 2.3 GPa

ISO 178 | 2 mm/min

Flexural yield strength

23.0 °C

90 MPa

Show Material materials with Flexural yield strength of 90 MPa

ISO 178 | 2 mm/min

Hardness, Ball Indentation

23.0 °C

95 MPa

Show Material materials with Hardness, Ball Indentation of 95 MPa

ISO 2039-1

Impact strength, Charpy notched

-30.0 °C

12 kJ/m²

Show Material materials with Impact strength, Charpy notched of 12 kJ/m²

ISO 179/1eA

23.0 °C

65 kJ/m²

Show Material materials with Impact strength, Charpy notched of 65 kJ/m²

ISO 179/1eA

Impact strength, Izod notched

-30.0 °C

15 kJ/m²

Show Material materials with Impact strength, Izod notched of 15 kJ/m²

ISO 180/1A

23.0 °C

65 kJ/m²

Show Material materials with Impact strength, Izod notched of 65 kJ/m²

ISO 180/1A

Unlock all property charts

Tensile strength

23.0 °C

69 MPa

Show Material materials with Tensile strength of 69 MPa

ISO 527 | 50 mm/min

Yield strength

23.0 °C

62 MPa

Show Material materials with Yield strength of 62 MPa

ISO 527 | 50 mm/min

Impact strength, Charpy unnotched

No Break @ 23,-30°C | ISO 179/1eU

Impact strength, Izod unnotched

No Break @ 23,-30°C| ISO 180/1U

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 7E-5 1/K

ISO 11359-2 | -23°C to 80°C

Heat deflection temperature, 1.80 MPa

122 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 122 °C

ISO 75/Ae | 1.8 MPa

Relative temperature index, electrical

130 °C

Show Material materials with Relative temperature index, electrical of 130 °C

UL 746B

Relative temperature index, mechanical impact

125 °C

Show Material materials with Relative temperature index, mechanical impact of 125 °C

UL 746B

Relative temperature index, mechanical strength

125 °C

Show Material materials with Relative temperature index, mechanical strength of 125 °C

UL 746B

Thermal conductivity

23.0 °C

0.2 W/(m·K)

Show Material materials with Thermal conductivity of 0.2 W/(m·K)

ISO 8302

Vicat softening temperature

141 °C

Show Material materials with Vicat softening temperature of 141 °C

ISO 306 | Rate B/120

Flammability

UL Compliant, 94V-2 Flame Class Rating | 0.8mm | UL 94 by SABIC-IP

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

250 V

Show Material materials with Comparative tracking index of 250 V

IEC 60112

Dielectric constant

23.0 °C

2.7 [-]

Show Material materials with Dielectric constant of 2.7 [-]

IEC 60250 | at 50/60 Hz

Dielectric strength

23.0 °C

17 kV/mm

Show Material materials with Dielectric strength of 17 kV/mm

IEC 60243-1 | in oil, 3.2 mm

Dissipation factor

23.0 °C

0.01 [-]

Show Material materials with Dissipation factor of 0.01 [-]

IEC 60250 | at 1 MHz

Optical

PropertyValueComment

Refractive index

1.59 [-]

Show Material materials with Refractive index of 1.59 [-]

ISO 489

Rheological Properties

PropertyTemperatureValueComment

Melt volume-flow rate

18 cm³/10min

Show Material materials with Melt volume-flow rate of 18 cm³/10min

ISO 1133 | 300°C/1.2 kg

Shrinkage

23.0 °C

0.5 - 0.7 %

Show Material materials with Shrinkage of 0.5 - 0.7 %

SABIC method

Technological properties

Property
Application areas

Electronic Components,Enclosure/Housing/Cover,Enclosures,LED Lighting,Personal Computing,Power Manangement,Small Appliance

Processing methods

Drying Temperature: 120°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 280-300°C, Nozzle Temperature: 270-290°C, Front - Zone 3 Temperature: 280-300°C, Middle - Zone 2 Temperature: 270-290°C, Rear - Zone 1 Temperature: 260-280°C, Hopper Temperature: 60-80°C, Mold Temperature: 80-100°C