SABIC® PC Resin PC2203R

Want to keep this datasheet? Save it now in your required format

Description

PC2203R resin is a high flow (MFR = 22 at 300?C/1.2kg), heat and UV stabilized, polycarbonate product with mold release designed for use in the general purpose molding market.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Bulk density

23.0 °C

1.2E-3 g/cm³

Show Material materials with Bulk density of 1.2E-3 g/cm³

ISO 1183

Density

23.0 °C

1.2 g/cm³

Show Material materials with Density of 1.2 g/cm³

ASTM D 792

Water absorption

23.0 °C

0.35 %

Show Material materials with Water absorption of 0.35 %

ISO 62

Water absorption, equilibrium

23.0 °C

0.35 %

Show Material materials with Water absorption, equilibrium of 0.35 %

ASTM D 570

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.35 GPa

Show Material materials with Elastic modulus of 2.35 GPa

ASTM D 638 | 50 mm/min

Elongation at yield

23.0 °C

6 %

Show Material materials with Elongation at yield of 6 %

ASTM D 638 | Type I, 50 mm/min

Flexural modulus

23.0 °C

2.3 GPa

Show Material materials with Flexural modulus of 2.3 GPa

ISO 178 | 2 mm/min

Flexural yield strength

23.0 °C

90 MPa

Show Material materials with Flexural yield strength of 90 MPa

ISO 178 | 2 mm/min

Hardness, Rockwell R

23.0 °C

120 [-]

Show Material materials with Hardness, Rockwell R of 120 [-]

ASTM D 785

Impact strength, Izod notched

-30.0 °C

12 kJ/m²

Show Material materials with Impact strength, Izod notched of 12 kJ/m²

ISO 180/1A

23.0 °C

65 kJ/m²

Show Material materials with Impact strength, Izod notched of 65 kJ/m²

ISO 180/1A

Impact strength, Izod notched, ASTM

23.0 °C

640 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 640 J/m

ASTM D 256

Yield strength

23.0 °C

63 MPa

Show Material materials with Yield strength of 63 MPa

ASTM D 638 | Type I, 50 mm/min

Impact strength, Izod unnotched

No Break @ 23,-30°C| ISO 180/1U

Impact strength, Izod unnotched, ASTM

No break @ 23°C | ASTM D 4812

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 7E-5 1/K

ASTM E 831 | -40°C to 95°C

Heat deflection temperature, 0.45 MPa

133 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 133 °C

ISO 75/Bf | 0.45 MPa

Thermal conductivity

23.0 °C

0.2 W/(m·K)

Show Material materials with Thermal conductivity of 0.2 W/(m·K)

ISO 8302

Vicat softening temperature

140 °C

Show Material materials with Vicat softening temperature of 140 °C

ASTM D 1525 | Rate B/50

Flammability

UL Recognized, 94V-2 Flame Class Rating | 0.75mm | UL 94

Electrical

PropertyTemperatureValueComment

Dielectric constant

23.0 °C

3 [-]

Show Material materials with Dielectric constant of 3 [-]

ASTM D 150 | at 1 MHz

Dielectric strength

23.0 °C

27 kV/mm

Show Material materials with Dielectric strength of 27 kV/mm

ASTM D 149 | 1.6 mm

Dissipation factor

23.0 °C

0.01 [-]

Show Material materials with Dissipation factor of 0.01 [-]

ASTM D 150 | at 1 MHz

Optical

PropertyValueComment

Refractive index

1.59 [-]

Show Material materials with Refractive index of 1.59 [-]

ISO 489

Transmission

88 - 90 %

Show Material materials with Transmission of 88 - 90 %

ASTM D 1003 | 2.54 mm

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

22 g/10min

Show Material materials with Melt mass-flow rate of 22 g/10min

ASTM D 1238 | 300°C/1.2 kg

Melt volume-flow rate

21 cm³/10min

Show Material materials with Melt volume-flow rate of 21 cm³/10min

ISO 1133 | 300°C/1.2 kg

Shrinkage

23.0 °C

0.5 - 0.7 %

Show Material materials with Shrinkage of 0.5 - 0.7 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Multi purpose injection moulding

Processing methods

Drying Temperature: 120°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 280-300°C, Nozzle Temperature: 270-290°C, Front - Zone 3 Temperature: 280-300°C, Middle - Zone 2 Temperature: 270-290°C, Rear - Zone 1 Temperature: 260-280°C, Hopper Temperature: 60-80°C, Mold Temperature: 80-100°C