Description

VALOX V3900WX is an unreinforced, UV stabilized, weatherable, impact modified flame retardant Polybutylene Terephthalate/Polycarbonate (PBT) injection moldable grade. It has excellent chemical resistance and a UL94V0@1.5mm and 5VA@3.0mm flame rating. This is an excellent candidate for a wide variety of applications including outdoor enclosures requiring UL746C F1 weatherability performance.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.3 g/cm³

Show Material materials with Density of 1.3 g/cm³

ASTM D 792

Water absorption

23.0 °C

0.03 %

Show Material materials with Water absorption of 0.03 %

ISO 62 | 23°C, 50% RH

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.2 GPa

Show Material materials with Elastic modulus of 2.2 GPa

ASTM D 638 | 5 mm/min

Elongation

23.0 °C

50 %

Show Material materials with Elongation of 50 %

ASTM D 638 | Type I, 50 mm/min

Elongation at yield

23.0 °C

5 %

Show Material materials with Elongation at yield of 5 %

ASTM D 638 | Type I, 50 mm/min

Flexural modulus

23.0 °C

2.13 GPa

Show Material materials with Flexural modulus of 2.13 GPa

ISO 178 | 2 mm/min

Flexural yield strength

23.0 °C

73 MPa

Show Material materials with Flexural yield strength of 73 MPa

ISO 178 | 2 mm/min

Impact strength, Charpy notched

23.0 °C

52 kJ/m²

Show Material materials with Impact strength, Charpy notched of 52 kJ/m²

ISO 179/1eA

Impact strength, Izod notched

-30.0 °C

8 kJ/m²

Show Material materials with Impact strength, Izod notched of 8 kJ/m²

ISO 180/1A

23.0 °C

15 - 45 kJ/m²

Show Material materials with Impact strength, Izod notched of 15 - 45 kJ/m²

ISO 180/1A

Impact strength, Izod notched, ASTM

-30.0 °C

110 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 110 J/m

ASTM D 256

23.0 °C

800 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 800 J/m

ASTM D 256

Unlock all property charts

Tensile strength

23.0 °C

43 MPa

Show Material materials with Tensile strength of 43 MPa

ASTM D 638 | Type I, 50 mm/min

Yield strength

23.0 °C

53 MPa

Show Material materials with Yield strength of 53 MPa

ASTM D 638 | Type I, 50 mm/min

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

8.84E-5 1/K

Show Material materials with Coefficient of thermal expansion of 8.84E-5 1/K

ASTM E 831 | -40°C to 40°C

Coefficient of thermal expansion, transverse

23.0 °C

8.97E-5 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 8.97E-5 1/K

ASTM E 831 | -40°C to 40°C

Heat deflection temperature, 1.80 MPa

75 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 75 °C

ASTM D 648 | 1.82 MPa, 3.2mm, unannealed

Relative temperature index, electrical

120 °C

Show Material materials with Relative temperature index, electrical of 120 °C

UL 746B

Relative temperature index, mechanical impact

120 °C

Show Material materials with Relative temperature index, mechanical impact of 120 °C

UL 746B

Relative temperature index, mechanical strength

120 °C

Show Material materials with Relative temperature index, mechanical strength of 120 °C

UL 746B

Vicat softening temperature

105 °C

Show Material materials with Vicat softening temperature of 105 °C

ASTM D 1525 | Rate B/50

Flammability

UL Compliant, 94-5VA Rating | 3mm | UL 94 by SABIC-IP

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

35 g/10min

Show Material materials with Melt mass-flow rate of 35 g/10min

ASTM D 1238 | 266°C/5.0 kg

Melt viscosity

260.0 °C

260 Pa·s

Show Material materials with Melt viscosity of 260 Pa·s

ISO 11443 | 1500 sec⁻¹

Melt volume-flow rate

11 cm³/10min

Show Material materials with Melt volume-flow rate of 11 cm³/10min

ISO 1133 | 265°C/2.16 kg

Shrinkage

23.0 °C

0.7 - 1 %

Show Material materials with Shrinkage of 0.7 - 1 %

SABIC method | 3.2 mm

Technological properties

Property
Application areas

Amusement Machine,ATM/Ticket Machine,Building Accessory,Circuit Protection,City,Cluster,Data Management,Data Transfer,Displays,Document Handling,Electronic Components,Enclosure/Housing/Cover,Enclosures,Energy Management,EV Infrastructure,Fluid Delivery,Gas/Electric Oven,Heavy Vehicles,Industrial Material Handling,Lawn/Garden,LED Lighting,Medical Device,Medical Facility Infrastructure,Meter Water,Monitoring and Imaging,Non-LED Lighting,Oil/Gas,Personal Computing,Pharmaceutical Manufacturing,Photovoltaic Components,Power Manangement,Respiratory,Security/Detection,Small Appliance,Surgical Devices,Water Treatment/Filtration,Wireless Communications,Wiring Devices,Wire & cable

Processing methods

Drying Temperature: 120°C, Drying Time: 3-4hrs, Drying Time (Cumulative): 12hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 250-265°C, Nozzle Temperature: 245-260°C, Front - Zone 3 Temperature: 250-265°C, Middle - Zone 2 Temperature: 245-260°C, Rear - Zone 1 Temperature: 240-255°C, Mold Temperature: 65-90°C, Back Pressure: 0.3-0.7MPa, Screw Speed: 50-80rpm, Shot to Cylinder Size: 40-80%, Vent Depth: 0.025-0.038mm