CYCOLOY™ Resin XCY620

Want to keep this datasheet? Save it now in your required format

Description

PC/ABS, hydrolytically stable, colors.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.14 g/cm³

Show Material materials with Density of 1.14 g/cm³

ASTM D 792

Water absorption

23.0 °C

0.15 %

Show Material materials with Water absorption of 0.15 %

ISO 62 | 23°C, 50% RH

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.3 GPa

Show Material materials with Elastic modulus of 2.3 GPa

ASTM D 638 | 5 mm/min

Elongation

23.0 °C

115 %

Show Material materials with Elongation of 115 %

ASTM D 638 | Type I, 50 mm/min

Elongation at yield

23.0 °C

4.7 %

Show Material materials with Elongation at yield of 4.7 %

ASTM D 638 | Type I, 50 mm/min

Flexural modulus

23.0 °C

2.2 GPa

Show Material materials with Flexural modulus of 2.2 GPa

ISO 178 | 2 mm/min

Flexural yield strength

23.0 °C

83 MPa

Show Material materials with Flexural yield strength of 83 MPa

ISO 178 | 2 mm/min

Impact strength, Charpy notched

-30.0 °C

45 kJ/m²

Show Material materials with Impact strength, Charpy notched of 45 kJ/m²

ISO 179/1eA

23.0 °C

60 kJ/m²

Show Material materials with Impact strength, Charpy notched of 60 kJ/m²

ISO 179/1eA

Impact strength, Izod notched

-30.0 °C

45 kJ/m²

Show Material materials with Impact strength, Izod notched of 45 kJ/m²

ISO 180/1A

23.0 °C

55 kJ/m²

Show Material materials with Impact strength, Izod notched of 55 kJ/m²

ISO 180/1A

Unlock all property charts

Impact strength, Izod notched, ASTM

-30.0 °C

480 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 480 J/m

ASTM D 256

23.0 °C

640 J/m

Show Material materials with Impact strength, Izod notched, ASTM of 640 J/m

ASTM D 256

Unlock all property charts

Tensile strength

23.0 °C

52 MPa

Show Material materials with Tensile strength of 52 MPa

ASTM D 638 | Type I, 50 mm/min

Yield strength

23.0 °C

55 MPa

Show Material materials with Yield strength of 55 MPa

ASTM D 638 | Type I, 50 mm/min

Impact strength, Charpy unnotched

No break @ 23,-30°C | ISO 179/1eU

Impact strength, Izod unnotched

No break @ 23,-30°C | ISO 180/1U

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

7E-5 1/K

Show Material materials with Coefficient of thermal expansion of 7E-5 1/K

ASTM E 831 | -40°C to 40°C

Coefficient of thermal expansion, transverse

23.0 °C

7E-5 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 7E-5 1/K

ASTM E 831 | -40°C to 40°C

Heat deflection temperature, 0.45 MPa

126 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 126 °C

ISO 75/Bf | 0.45 MPa

Thermal conductivity

23.0 °C

0.2 W/(m·K)

Show Material materials with Thermal conductivity of 0.2 W/(m·K)

ISO 8302

Vicat softening temperature

127 °C

Show Material materials with Vicat softening temperature of 127 °C

ASTM D 1525 | Rate B/50

Electrical

PropertyTemperatureValueComment

Dielectric strength

23.0 °C

17 kV/mm

Show Material materials with Dielectric strength of 17 kV/mm

IEC 60243-1 | in oil, 3.2 mm

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

22 g/10min

Show Material materials with Melt mass-flow rate of 22 g/10min

ASTM D 1238 | 260°C/5.0 kgf

Melt viscosity

260.0 °C

195 Pa·s

Show Material materials with Melt viscosity of 195 Pa·s

ISO 11443 | 1500 sec⁻¹

Melt volume-flow rate

18 cm³/10min

Show Material materials with Melt volume-flow rate of 18 cm³/10min

ISO 1133 | 260°C/5.0 kg

Shrinkage

23.0 °C

0.5 - 0.7 %

Show Material materials with Shrinkage of 0.5 - 0.7 %

SABIC method | 3.2 mm

Shrinkage, transverse

23.0 °C

0.5 - 0.7 %

Show Material materials with Shrinkage, transverse of 0.5 - 0.7 %

SABIC method

Technological properties

Property
Application areas

Applique,Audio,Auto Aftermarket,Cluster,Console,Data Transfer,Displays,Document Handling,Doors Hardware/Trim,Electronic Components,Enclosure/Housing/Cover,Enclosures,Energy Management,EV Infrastructure,Exterior Mirror,Exterior Rail Components,Exterior Trim,Forward Lighting,Front End,Front Grille,Glove Box,Headliner,Heavy Vehicles,Infotainment/Telematic,Interior,Meter Gas,Motorcycle,Non-LED Lighting,Overhead,Personal Computing,Personal Water Craft,Rail,Rear/Signal Lighting,Recreational Vehicle,Seat,Spoiler,Structure,Trim,Water Treatment/Filtration

Processing methods

Drying Temperature: 95-105°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 260-290°C, Nozzle Temperature: 240-280°C, Front - Zone 3 Temperature: 250-290°C, Middle - Zone 2 Temperature: 250-290°C, Rear - Zone 1 Temperature: 230-260°C, Hopper Temperature: 60-80°C, Mold Temperature: 60-90°C