Description

Common features of Crastin® thermoplastic polyester resin include mechanical and physical properties such as stiffness and toughness, heat resistance, friction and wear resistance, excellent surface finishes and good colourability. Crastin® thermoplastic polyester resin has excellent electrical insulation characteristics and high arc-resistant grades are available. Many flame retardant grades have UL recognition (class V-0). Crastin® thermoplastic polyester resin typically has high chemical and heat ageing resistance. The good melt stability of Crastin® thermoplastic polyester resin normally enables the recycling of properly handled production waste.If recycling is not possible, DuPont recommends, as the preferred option, incineration with energy recovery (-24 kJ/g of base polymer) in appropriately equipped installations. For disposal, local regulations have to be observed. Crastin® thermoplastic polyester resin typically is used in demanding applications in the electronics, electrical, automotive, mechanical engineering, chemical, domestic appliances and sporting goods industry.Crastin® S600F20 NC010 is an unreinforced, lubricated, medium viscosity polybutylene terephthalate resin for injection molding.

Equivalent Materials

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Coefficient of friction

0.4 [-]

Show Material materials with Coefficient of friction of 0.4 [-]

ASTM 1894 | against steel

Density

23.0 °C

1.31 g/cm³

Show Material materials with Density of 1.31 g/cm³

ISO 1183

Water absorption

23.0 °C

0.4 %

Show Material materials with Water absorption of 0.4 %

Sim. to ISO 62 | 80mil

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

2.5 GPa

Show Material materials with Elastic modulus of 2.5 GPa

ISO 527-1/-2

Elongation

23.0 °C

40 %

Show Material materials with Elongation of 40 %

ISO 527-1/-2

Elongation at yield

23.0 °C

4 %

Show Material materials with Elongation at yield of 4 %

ISO 527-1/-2

Flexural modulus

23.0 °C

2.2 GPa

Show Material materials with Flexural modulus of 2.2 GPa

ISO 178

Flexural strength

23.0 °C

85 MPa

Show Material materials with Flexural strength of 85 MPa

ISO 178

Hardness, Ball Indentation

23.0 °C

139 MPa

Show Material materials with Hardness, Ball Indentation of 139 MPa

ISO 2039-1

Impact strength, Charpy notched

-6.0 °C

4 kJ/m²

Show Material materials with Impact strength, Charpy notched of 4 kJ/m²

ISO 179/1eA

23.0 °C

5 kJ/m²

Show Material materials with Impact strength, Charpy notched of 5 kJ/m²

ISO 179/1eA

Impact strength, Izod unnotched

23.0 °C

4.5 kJ/m²

Show Material materials with Impact strength, Izod unnotched of 4.5 kJ/m²

ISO 180/1A

Poisson's ratio

23.0 °C

0.38 [-]

Show Material materials with Poisson's ratio of 0.38 [-]

Yield strength

23.0 °C

55 MPa

Show Material materials with Yield strength of 55 MPa

ISO 527-1/-2

Impact strength, Charpy unnotched

No Break @ 23,-6°C, ISO 179/1eA

Impact strength, Izod notched

No Break @ 23°C, ISO 179/1eU

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.9E-4 1/K

Show Material materials with Coefficient of thermal expansion of 1.9E-4 1/K

ISO 11359-1/-2 | 23 - 55°C

Coefficient of thermal expansion, transverse

23.0 °C

2E-4 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 2E-4 1/K

ISO 11359-1/-2 | 55 - 160°C

Glass transition temperature

55 °C

Show Material materials with Glass transition temperature of 55 °C

ISO 11357-1/-2 | 18°F/min

Heat deflection temperature, 0.45 MPa

180 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 180 °C

ISO 75-1/-2 | annealed

Heat deflection temperature, 1.80 MPa

60 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 60 °C

ISO 75-1/-2 | annealed

Melting point

225 °C

Show Material materials with Melting point of 225 °C

ISO 11357-1/-3 | 18°F/min

Relative temperature index, electrical

130 °C

Show Material materials with Relative temperature index, electrical of 130 °C

UL 746B | 240mil

Relative temperature index, mechanical impact

115 °C

Show Material materials with Relative temperature index, mechanical impact of 115 °C

UL 746B | 240mil

Relative temperature index, mechanical strength

120 °C

Show Material materials with Relative temperature index, mechanical strength of 120 °C

UL 746B | 240mil

Specific heat capacity

23.0 °C

2110 J/(kg·K)

Show Material materials with Specific heat capacity of 2110 J/(kg·K)

of melt

Thermal conductivity

23.0 °C

0.29 W/(m·K)

Show Material materials with Thermal conductivity of 0.29 W/(m·K)

of solid

Vicat softening temperature

175 °C

Show Material materials with Vicat softening temperature of 175 °C

ISO 306 | 90°F/h, 11 lbf

Flammability

Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: HB class, Thickness tested: 0.75 mm, UL recognition: yes -, Oxygen index: 22 %, Glow Wire Flammability Index, 120mil: 750 °C, Glow Wire Ignition Temperature, 30mil: 750 °C, Glow Wire Ignition Temperature, 40mil: 750 °C, Glow Wire Ignition Temperature, 60mil: 750 °C, Glow Wire Ignition Temperature, 80mil: 750 °C, Glow Wire Ignition Temperature, 120mil: 725 °C, FMVSS Class: SE -

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

575 V

Show Material materials with Comparative tracking index of 575 V

IEC 60112

Dielectric constant, 100Hz

23.0 °C

3.6 [-]

Show Material materials with Dielectric constant, 100Hz of 3.6 [-]

IEC 62631-2-1

Dielectric constant, 1MHz

23.0 °C

3.2 [-]

Show Material materials with Dielectric constant, 1MHz of 3.2 [-]

IEC 62631-2-1

Dielectric strength

23.0 °C

26 kV/mm

Show Material materials with Dielectric strength of 26 kV/mm

IEC 60243-1

Dissipation factor, 100Hz

23.0 °C

7.9E-4 [-]

Show Material materials with Dissipation factor, 100Hz of 7.9E-4 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

0.02 [-]

Show Material materials with Dissipation factor, 1MHz of 0.02 [-]

IEC 62631-2-1

Surface resistivity

23.0 °C

1.00E+12 Ω/sq

Show Material materials with Surface resistivity of 1.00E+12 Ω/sq

IEC 62631-3-2

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Material materials with Volume resistivity of 1.00E+15 Ω·cm

min. | IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

19 g/10min

Show Material materials with Melt mass-flow rate of 19 g/10min

ISO 1133 | 250°C/2.16kg

Melt volume-flow rate

14 cm³/10min

Show Material materials with Melt volume-flow rate of 14 cm³/10min

ISO 1133

Shrinkage

23.0 °C

1.7 %

Show Material materials with Shrinkage of 1.7 %

ISO 294-4, 2577

Shrinkage, transverse

23.0 °C

1.6 %

Show Material materials with Shrinkage, transverse of 1.6 %

ISO 294-4, 2577

Technological properties

Property
Processing methods

Drying Recommended: yes, Drying Temperature: 120°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.04%, Melt Temperature Optimum: 250°C, Min. melt temperature: 240°C, Max. melt temperature: 260°C, Mold Temperature Optimum: 80°C, Min. mold temperature: 30°C, Max. mold temperature: 130°C, Hold pressure range: ≥60MPa, Hold pressure time: 4s/mm, Back pressure: As low as possible, Ejection temperature: 170°C