Delrin® 100 BK602

Want to keep this datasheet? Save it now in your required format

Description

Common features of Delrin® acetal resins include mechanical and physical properties such as high mechanical strength and rigidity, excellent fatigue and impact resistance, as well as resistance to moisture, gasoline, lubricants, solvents, and many other neutral chemicals. Delrin® acetal resins also have excellent dimensional stability and good electrical insulating characteristics. They are naturally resilient, self-lubricating, and available in a variety of colors and speciality grades. Delrin® acetal resin typically is used in demanding applications in the automotive, domestic appliances, sports, industrial engineering, electronics, and consumer goods industries.Delrin® 100 is a high viscosity acetal homopolymer for use in easy-to-fill molds. Delrin® 100 provides optimum mechanical performance with its excellent combination of toughness and strength.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.42 g/cm³

Show Material materials with Density of 1.42 g/cm³

ISO 1183

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

3.15 GPa

Show Material materials with Elastic modulus of 3.15 GPa

ISO 527-1/-2

Elongation

23.0 °C

500 %

Show Material materials with Elongation of 500 %

min. | ISO 527-1/-2

Elongation at yield

23.0 °C

23 %

Show Material materials with Elongation at yield of 23 %

ISO 527-1/-2

Flexural modulus

23.0 °C

2.9 GPa

Show Material materials with Flexural modulus of 2.9 GPa

ISO 178

Hardness, Rockwell M

23.0 °C

91 [-]

Show Material materials with Hardness, Rockwell M of 91 [-]

ISO 2039-2

Hardness, Rockwell R

23.0 °C

121 [-]

Show Material materials with Hardness, Rockwell R of 121 [-]

ISO 2039-2

Impact strength, Charpy notched

-6.0 °C

10.5 kJ/m²

Show Material materials with Impact strength, Charpy notched of 10.5 kJ/m²

ISO 179/1eA

23.0 °C

12 kJ/m²

Show Material materials with Impact strength, Charpy notched of 12 kJ/m²

ISO 179/1eA

Impact strength, Charpy unnotched

-6.0 °C

350 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 350 kJ/m²

No Break @ 23°C, ISO 179/1eU

Impact strength, Izod unnotched

-40.0 °C

10 kJ/m²

Show Material materials with Impact strength, Izod unnotched of 10 kJ/m²

ISO 180/1A

23.0 °C

11 kJ/m²

Show Material materials with Impact strength, Izod unnotched of 11 kJ/m²

ISO 180/1A

Unlock all property charts

Poisson's ratio

23.0 °C

0.37 [-]

Show Material materials with Poisson's ratio of 0.37 [-]

Yield strength

23.0 °C

72 MPa

Show Material materials with Yield strength of 72 MPa

ISO 527-1/-2

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1E-4 1/K

Show Material materials with Coefficient of thermal expansion of 1E-4 1/K

ISO 11359-1/-2 | -40 - 23°C

Coefficient of thermal expansion, transverse

23.0 °C

1E-4 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 1E-4 1/K

ISO 11359-1/-2 | -40 - 23°C

Heat deflection temperature, 1.80 MPa

97 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 97 °C

ISO 75-1/-2

Melting point

178 °C

Show Material materials with Melting point of 178 °C

ISO 11357-1/-3 | 18°F/min

Relative temperature index, electrical

105 °C

Show Material materials with Relative temperature index, electrical of 105 °C

UL 746B | 240mil

Relative temperature index, mechanical impact

85 °C

Show Material materials with Relative temperature index, mechanical impact of 85 °C

UL 746B | 240mil

Relative temperature index, mechanical strength

90 °C

Show Material materials with Relative temperature index, mechanical strength of 90 °C

UL 746B | 240mil

Vicat softening temperature

175 °C

Show Material materials with Vicat softening temperature of 175 °C

ISO 306 | 90°F, 2 lbf

Flammability

Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: HB class, Thickness tested: 0.8 mm, UL recognition: yes -, FMVSS Class: B -, Burning rate, Thickness 1 mm: 37 mm/min

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

600 V

Show Material materials with Comparative tracking index of 600 V

IEC 60112

Dielectric constant, 100Hz

23.0 °C

4 [-]

Show Material materials with Dielectric constant, 100Hz of 4 [-]

IEC 62631-2-1

Dielectric constant, 1MHz

23.0 °C

3.9 [-]

Show Material materials with Dielectric constant, 1MHz of 3.9 [-]

IEC 62631-2-1

Dielectric strength

23.0 °C

45 kV/mm

Show Material materials with Dielectric strength of 45 kV/mm

IEC 60243-1

Dissipation factor, 100Hz

23.0 °C

5E-4 [-]

Show Material materials with Dissipation factor, 100Hz of 5E-4 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

6E-3 [-]

Show Material materials with Dissipation factor, 1MHz of 6E-3 [-]

IEC 62631-2-1

Surface resistivity

23.0 °C

1.00E+15 Ω/sq

Show Material materials with Surface resistivity of 1.00E+15 Ω/sq

min. | IEC 62631-3-2

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Material materials with Volume resistivity of 1.00E+15 Ω·cm

min. | IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

2.4 g/10min

Show Material materials with Melt mass-flow rate of 2.4 g/10min

ISO 1133 | 190°C/2.16kg

Melt volume-flow rate

2 cm³/10min

Show Material materials with Melt volume-flow rate of 2 cm³/10min

ISO 1133

Shrinkage

23.0 °C

2.2 %

Show Material materials with Shrinkage of 2.2 %

ISO 294-4, 2577

Shrinkage, transverse

23.0 °C

1.8 %

Show Material materials with Shrinkage, transverse of 1.8 %

ISO 294-4, 2577

Technological properties

Property
Processing methods

Drying Recommended: yes, Drying Temperature: 80°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.2%, Melt Temperature Optimum: 215°C, Min. melt temperature: 210°C, Max. melt temperature: 220°C, Max. screw tangential speed: 0.2m/s, Mold Temperature Optimum: 90°C, Min. mold temperature: 80°C, Max. mold temperature: 100°C, Hold pressure range: 90-110MPa, Hold pressure time: 8s/mm