Crastin® SK605 NC010

Alternative and trade names
PBT-GF30
Want to keep this datasheet? Save it now in your required format

Description

Common features of Crastin® thermoplastic polyester resin include mechanical and physical properties such as stiffness and toughness, heat resistance, friction and wear resistance, excellent surface finishes and good colourability. Crastin® thermoplastic polyester resin has excellent electrical insulation characteristics and high arc-resistant grades are available. Many flame retardant grades have UL recognition (class V-0). Crastin® thermoplastic polyester resin typically has high chemical and heat ageing resistance. The good melt stability of Crastin® thermoplastic polyester resin normally enables the recycling of properly handled production waste.If recycling is not possible, DuPont recommends, as the preferred option, incineration with energy recovery (-24 kJ/g of base polymer) in appropriately equipped installations. For disposal, local regulations have to be observed. Crastin® thermoplastic polyester resin typically is used in demanding applications in the electronics, electrical, automotive, mechanical engineering, chemical, domestic appliances and sporting goods industry.Crastin® SK605 NC010 is a 30% glass fiber reinforced, lubricated polybutylene terephthalate resin for injection molding.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.53 g/cm³

Show Material materials with Density of 1.53 g/cm³

ISO 1183

Water absorption

23.0 °C

0.35 %

Show Material materials with Water absorption of 0.35 %

Sim. to ISO 62 | 80mil

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

10 GPa

Show Material materials with Elastic modulus of 10 GPa

ISO 527-1/-2

Elongation

23.0 °C

2.7 %

Show Material materials with Elongation of 2.7 %

ISO 527-1/-2

Flexural modulus

23.0 °C

9 GPa

Show Material materials with Flexural modulus of 9 GPa

ISO 178

Flexural strength

23.0 °C

200 MPa

Show Material materials with Flexural strength of 200 MPa

ISO 178

Hardness, Ball Indentation

23.0 °C

205 MPa

Show Material materials with Hardness, Ball Indentation of 205 MPa

ISO 2039-1

Impact strength, Charpy notched

-40.0 °C

10 kJ/m²

Show Material materials with Impact strength, Charpy notched of 10 kJ/m²

ISO 179/1eA

-6.0 °C

11 kJ/m²

Show Material materials with Impact strength, Charpy notched of 11 kJ/m²

ISO 179/1eA

23.0 °C

10 kJ/m²

Show Material materials with Impact strength, Charpy notched of 10 kJ/m²

ISO 179/1eA

Impact strength, Charpy unnotched

-40.0 °C

75 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 75 kJ/m²

ISO 179/1eU

-6.0 °C

75 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 75 kJ/m²

ISO 179/1eU

23.0 °C

70 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 70 kJ/m²

ISO 179/1eU

Unlock all property charts

Impact strength, Izod notched

-40.0 °C

55 kJ/m²

Show Material materials with Impact strength, Izod notched of 55 kJ/m²

ISO 180/1U

-30.0 °C

55 kJ/m²

Show Material materials with Impact strength, Izod notched of 55 kJ/m²

ISO 180/1U

23.0 °C

60 kJ/m²

Show Material materials with Impact strength, Izod notched of 60 kJ/m²

ISO 180/1U

Unlock all property charts

Impact strength, Izod unnotched

-40.0 °C

10 kJ/m²

Show Material materials with Impact strength, Izod unnotched of 10 kJ/m²

ISO 180/1A

-30.0 °C

10 kJ/m²

Show Material materials with Impact strength, Izod unnotched of 10 kJ/m²

ISO 180/1A

23.0 °C

11 kJ/m²

Show Material materials with Impact strength, Izod unnotched of 11 kJ/m²

ISO 180/1A

Unlock all property charts

Poisson's ratio

23.0 °C

0.34 [-]

Show Material materials with Poisson's ratio of 0.34 [-]

Tensile strength

23.0 °C

140 MPa

Show Material materials with Tensile strength of 140 MPa

ISO 527-1/-2

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

3E-5 1/K

Show Material materials with Coefficient of thermal expansion of 3E-5 1/K

ISO 11359-1/-2

Coefficient of thermal expansion, transverse

23.0 °C

9E-5 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 9E-5 1/K

ISO 11359-1/-2

Heat deflection temperature, 0.45 MPa

220 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 220 °C

ISO 75-1/-2

Heat deflection temperature, 1.80 MPa

205 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 205 °C

ISO 75-1/-2

Melting point

224 °C

Show Material materials with Melting point of 224 °C

ISO 11357-1/-3 | 18°F/min

Relative temperature index, electrical

130 °C

Show Material materials with Relative temperature index, electrical of 130 °C

UL 746B | 240mil

Relative temperature index, mechanical impact

130 °C

Show Material materials with Relative temperature index, mechanical impact of 130 °C

UL 746B | 240mil

Relative temperature index, mechanical strength

130 °C

Show Material materials with Relative temperature index, mechanical strength of 130 °C

UL 746B | 240mil

Specific heat capacity

23.0 °C

1730 J/(kg·K)

Show Material materials with Specific heat capacity of 1730 J/(kg·K)

of melt

Vicat softening temperature

215 °C

Show Material materials with Vicat softening temperature of 215 °C

ISO 306 | 90°F/h, 11 lbf

Flammability

Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: HB class, Thickness tested: 0.75 mm, UL recognition: yes -, Oxygen index: 19 %, Glow Wire Flammability Index, 30mil: 725 °C, Glow Wire Flammability Index, 60mil: 725 °C, Glow Wire Flammability Index, 120mil: 750 °C, Glow Wire Ignition Temperature, 30mil: 750 °C, Glow Wire Ignition Temperature, 40mil: 750 °C, Glow Wire Ignition Temperature, 60mil: 750 °C, Glow Wire Ignition Temperature, 80mil: 750 °C, Glow Wire Ignition Temperature, 120mil: 775 °C, FMVSS Class: B -, Burning rate, Thickness 1 mm: 41 mm/min

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

400 V

Show Material materials with Comparative tracking index of 400 V

IEC 60112

Dielectric constant, 100Hz

23.0 °C

3.9 [-]

Show Material materials with Dielectric constant, 100Hz of 3.9 [-]

IEC 62631-2-1

Dielectric constant, 1MHz

23.0 °C

3.8 [-]

Show Material materials with Dielectric constant, 1MHz of 3.8 [-]

IEC 62631-2-1

Dielectric strength

23.0 °C

17 kV/mm

Show Material materials with Dielectric strength of 17 kV/mm

IEC 60243-1 | Short Time, 2mm

Dissipation factor, 100Hz

23.0 °C

7.5E-4 [-]

Show Material materials with Dissipation factor, 100Hz of 7.5E-4 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

0.02 [-]

Show Material materials with Dissipation factor, 1MHz of 0.02 [-]

IEC 62631-2-1

Surface resistivity

23.0 °C

1.00E+15 Ω/sq

Show Material materials with Surface resistivity of 1.00E+15 Ω/sq

min. | IEC 62631-3-2

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Material materials with Volume resistivity of 1.00E+15 Ω·cm

min. | IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Melt mass-flow rate

10 g/10min

Show Material materials with Melt mass-flow rate of 10 g/10min

ISO 1133 | 250°C/2.16kg

Melt volume-flow rate

7 cm³/10min

Show Material materials with Melt volume-flow rate of 7 cm³/10min

ISO 1133

Shrinkage

23.0 °C

0.3 %

Show Material materials with Shrinkage of 0.3 %

ISO 294-4, 2577

Shrinkage, transverse

23.0 °C

1.1 %

Show Material materials with Shrinkage, transverse of 1.1 %

ISO 294-4, 2577

Technological properties

Property
Fillers

30% Glass Fiber

Processing methods

Drying Recommended: yes, Drying Temperature: 120°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.04%, Melt Temperature Optimum: 250°C, Min. melt temperature: 240°C, Max. melt temperature: 260°C, Mold Temperature Optimum: 80°C, Min. mold temperature: 30°C, Max. mold temperature: 130°C, Hold pressure range: ≥60MPa, Hold pressure time: 3s/mm, Back pressure: As low as possible, Ejection temperature: 170°C