Common features of Delrin® acetal resins include mechanical and physical properties such as high mechanical strength and rigidity, excellent fatigue and impact resistance, as well as resistance to moisture, gasoline, lubricants, solvents, and many other neutral chemicals. Delrin® acetal resins also have excellent dimensional stability and good electrical insulating characteristics. They are naturally resilient, self-lubricating, and available in a variety of colors and speciality grades. Delrin® acetal resin typically is used in demanding applications in the automotive, domestic appliances, sports, industrial engineering, electronics, and consumer goods industries.Delrin® 527UV is a UV-stabilized medium viscosity acetal homopolymer developed for applications in automotive interiors. It represents a dramatic improvement over Delrin® 507 in mechanical performance after prolonged UV exposure and thermal stability.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.42 g/cm³

Show Material materials with Density of 1.42 g/cm³

ISO 1183

Water absorption

23.0 °C

0.5 %

Show Material materials with Water absorption of 0.5 %

Sim. to ISO 62 | Immersion 24h

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

3.1 GPa

Show Material materials with Elastic modulus of 3.1 GPa

ISO 527-1/-2

Elongation

23.0 °C

30 %

Show Material materials with Elongation of 30 %

ISO 527-1/-2

Elongation at yield

23.0 °C

17 %

Show Material materials with Elongation at yield of 17 %

ISO 527-1/-2

Flexural modulus

23.0 °C

3 GPa

Show Material materials with Flexural modulus of 3 GPa

ISO 178

Flexural strength

23.0 °C

77 MPa

Show Material materials with Flexural strength of 77 MPa

ISO 178

Hardness, Rockwell M

23.0 °C

92 [-]

Show Material materials with Hardness, Rockwell M of 92 [-]

ISO 2039-2

Hardness, Rockwell R

23.0 °C

120 [-]

Show Material materials with Hardness, Rockwell R of 120 [-]

ISO 2039-2

Impact strength, Charpy notched

-6.0 °C

8 kJ/m²

Show Material materials with Impact strength, Charpy notched of 8 kJ/m²

ISO 179/1eA

23.0 °C

9 kJ/m²

Show Material materials with Impact strength, Charpy notched of 9 kJ/m²

ISO 179/1eA

Impact strength, Charpy unnotched

-6.0 °C

260 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 260 kJ/m²

ISO 179/1eU

23.0 °C

260 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 260 kJ/m²

ISO 179/1eU

Unlock all property charts

Impact strength, Izod unnotched

-40.0 °C

8 kJ/m²

Show Material materials with Impact strength, Izod unnotched of 8 kJ/m²

ISO 180/1A

23.0 °C

8 kJ/m²

Show Material materials with Impact strength, Izod unnotched of 8 kJ/m²

ISO 180/1A

Unlock all property charts

Poisson's ratio

23.0 °C

0.37 [-]

Show Material materials with Poisson's ratio of 0.37 [-]

Yield strength

23.0 °C

70 MPa

Show Material materials with Yield strength of 70 MPa

ISO 527-1/-2

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.1E-4 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-4 1/K

ISO 11359-1/-2

Coefficient of thermal expansion, transverse

23.0 °C

1.2E-4 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 1.2E-4 1/K

ISO 11359-1/-2

Heat deflection temperature, 0.45 MPa

163 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 163 °C

ISO 75-1/-2

Heat deflection temperature, 1.80 MPa

95 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 95 °C

ISO 75-1/-2

Melting point

178 °C

Show Material materials with Melting point of 178 °C

ISO 11357-1/-3 | 18°F/min

Relative temperature index, electrical

50 °C

Show Material materials with Relative temperature index, electrical of 50 °C

UL 746B | 30mil

Relative temperature index, mechanical impact

50 °C

Show Material materials with Relative temperature index, mechanical impact of 50 °C

UL 746B | 30mil

Relative temperature index, mechanical strength

50 °C

Show Material materials with Relative temperature index, mechanical strength of 50 °C

UL 746B | 30mil

Vicat softening temperature

174 °C

Show Material materials with Vicat softening temperature of 174 °C

ISO 306 | 90°F, 2 lbf

Flammability

Burning Behav. at thickness h: HB class, Thickness tested: 0.8 mm, UL recognition: yes -, FMVSS Class: B -, Burning rate, Thickness 1 mm: 21 mm/min

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

600 V

Show Material materials with Comparative tracking index of 600 V

IEC 60112

Dielectric constant, 100Hz

23.0 °C

3.8 [-]

Show Material materials with Dielectric constant, 100Hz of 3.8 [-]

IEC 62631-2-1

Dielectric constant, 1MHz

23.0 °C

3.8 [-]

Show Material materials with Dielectric constant, 1MHz of 3.8 [-]

IEC 62631-2-1

Dissipation factor, 100Hz

23.0 °C

2.1E-3 [-]

Show Material materials with Dissipation factor, 100Hz of 2.1E-3 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

5.6E-3 [-]

Show Material materials with Dissipation factor, 1MHz of 5.6E-3 [-]

IEC 62631-2-1

Surface resistivity

23.0 °C

2.00E+13 Ω/sq

Show Material materials with Surface resistivity of 2.00E+13 Ω/sq

IEC 62631-3-2

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Material materials with Volume resistivity of 1.00E+15 Ω·cm

min. | IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Melt volume-flow rate

13 cm³/10min

Show Material materials with Melt volume-flow rate of 13 cm³/10min

ISO 1133

Shrinkage

23.0 °C

2 %

Show Material materials with Shrinkage of 2 %

ISO 294-4, 2577

Shrinkage, transverse

23.0 °C

1.9 %

Show Material materials with Shrinkage, transverse of 1.9 %

ISO 294-4, 2577

Technological properties

Property
Processing methods

Drying Recommended: yes, Drying Temperature: 80°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.2%, Melt Temperature Optimum: 215°C, Min. melt temperature: 210°C, Max. melt temperature: 220°C, Mold Temperature Optimum: 90°C, Min. mold temperature: 80°C, Max. mold temperature: 100°C, Hold pressure range: 80-100MPa, Hold pressure time: 8s/mm