Rynite® FR515 NC010

Alternative and trade names
PET-GF15FR(17)
Want to keep this datasheet? Save it now in your required format

Description

Common features of Rynite® thermoplastic polyester include mechanical and physical properties such as excellent balance of strength and stiffness, dimensional stability, creep resistance, heat resistance,high surface gloss and good inherent electrical properties at elevated temperature. It can be processed over a broad temperature range and has excellent flow properties. Rynite® thermoplastic polyester resins aretypically used in demanding applications in the automotive, electrical and electronics, appliances where they successfully replace metals and thermosets, as well as other thermoplastic polymers. Rynite® FR515 NC010 is a 15% glass reinforced, flame retardant modified polyethylene terephthalate resin.

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.53 g/cm³

Show Material materials with Density of 1.53 g/cm³

ISO 1183

Mechanical

PropertyTemperatureValueComment

Compressive strength

23.0 °C

170 MPa

Show Material materials with Compressive strength of 170 MPa

ISO 604

Elastic modulus

23.0 °C

6.8 GPa

Show Material materials with Elastic modulus of 6.8 GPa

ISO 527-1/-2

Elongation

23.0 °C

2.6 %

Show Material materials with Elongation of 2.6 %

ISO 527-1/-2

Flexural modulus

23.0 °C

5.94 GPa

Show Material materials with Flexural modulus of 5.94 GPa

ISO 178

Flexural strength

23.0 °C

170 MPa

Show Material materials with Flexural strength of 170 MPa

ISO 178

Hardness, Rockwell M

23.0 °C

88 [-]

Show Material materials with Hardness, Rockwell M of 88 [-]

ISO 2039-2

Hardness, Rockwell R

23.0 °C

120 [-]

Show Material materials with Hardness, Rockwell R of 120 [-]

ISO 2039-2

Impact strength, Charpy notched

-40.0 °C

7 kJ/m²

Show Material materials with Impact strength, Charpy notched of 7 kJ/m²

ISO 179/1eA

-6.0 °C

7 kJ/m²

Show Material materials with Impact strength, Charpy notched of 7 kJ/m²

ISO 179/1eA

23.0 °C

8 kJ/m²

Show Material materials with Impact strength, Charpy notched of 8 kJ/m²

ISO 179/1eA

Impact strength, Charpy unnotched

-40.0 °C

20 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 20 kJ/m²

ISO 179/1eU

-6.0 °C

35 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 35 kJ/m²

ISO 179/1eU

23.0 °C

40 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 40 kJ/m²

ISO 179/1eU

Unlock all property charts

Poisson's ratio

23.0 °C

0.35 [-]

Show Material materials with Poisson's ratio of 0.35 [-]

Shear strength

23.0 °C

50 MPa

Show Material materials with Shear strength of 50 MPa

ASTM D 732

Tensile strength

23.0 °C

107 MPa

Show Material materials with Tensile strength of 107 MPa

ISO 527-1/-2

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

ISO 11359-1/-2 | 23 - 55°C

Coefficient of thermal expansion, transverse

23.0 °C

1E-4 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 1E-4 1/K

ISO 11359-1/-2 | 55 - 160°C

Heat deflection temperature, 0.45 MPa

240 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 240 °C

ISO 75-1/-2

Heat deflection temperature, 1.80 MPa

200 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 200 °C

ISO 75-1/-2

Melting point

254 °C

Show Material materials with Melting point of 254 °C

ISO 11357-1/-3 | 18°F/min

Relative temperature index, electrical

140 °C

Show Material materials with Relative temperature index, electrical of 140 °C

UL 746B | 120mil

Relative temperature index, mechanical impact

140 °C

Show Material materials with Relative temperature index, mechanical impact of 140 °C

UL 746B | 120mil

Relative temperature index, mechanical strength

140 °C

Show Material materials with Relative temperature index, mechanical strength of 140 °C

UL 746B | 120mil

Thermal conductivity

23.0 °C

0.25 W/(m·K)

Show Material materials with Thermal conductivity of 0.25 W/(m·K)

of solid

Vicat softening temperature

210 °C

Show Material materials with Vicat softening temperature of 210 °C

ISO 306 | 90°F/h, 11 lbf

Flammability

Burning Behav. at thickness h: V-0 class, Thickness tested: 0.86 mm, UL recognition: yes -, Burning Behav. 5V at thickness h: 5VA class, Thickness tested: 1.5 mm, UL recognition: yes -, Oxygen index: 32 %, Glow Wire Flammability Index, 120mil: 960 °C, Glow Wire Ignition Temperature, 120mil: 875 °C, Glow Wire Temperature, No Flame, 40mil: 750 °C, Glow Wire Temperature, No Flame, 80mil: 650 °C, FMVSS Class: B -, Burning rate, Thickness 1 mm: <80 mm/min

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

3 V

Show Material materials with Comparative tracking index of 3 V

UL 746A

Dielectric constant, 100Hz

23.0 °C

3.8 [-]

Show Material materials with Dielectric constant, 100Hz of 3.8 [-]

IEC 62631-2-1

Dielectric constant, 1MHz

23.0 °C

3.5 [-]

Show Material materials with Dielectric constant, 1MHz of 3.5 [-]

IEC 62631-2-1

Dielectric strength

23.0 °C

26 kV/mm

Show Material materials with Dielectric strength of 26 kV/mm

IEC 60243-1 | Short Time, 23°C, 2mm

Dissipation factor, 100Hz

23.0 °C

9E-3 [-]

Show Material materials with Dissipation factor, 100Hz of 9E-3 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

0.02 [-]

Show Material materials with Dissipation factor, 1MHz of 0.02 [-]

IEC 62631-2-1

Surface resistivity

23.0 °C

1.00E+13 Ω/sq

Show Material materials with Surface resistivity of 1.00E+13 Ω/sq

IEC 62631-3-2

Volume resistivity

23.0 °C

1.00E+15 Ω·cm

Show Material materials with Volume resistivity of 1.00E+15 Ω·cm

min. | IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

0.5 %

Show Material materials with Shrinkage of 0.5 %

ISO 294-4 | Annealed

Shrinkage, transverse

23.0 °C

1.15 %

Show Material materials with Shrinkage, transverse of 1.15 %

ISO 294-4 | Annealed

Technological properties

Property
Fillers

15% Glass Fiber

Processing methods

Drying Recommended: yes, Drying Temperature: 120°C, Drying Time, Dehumidified Dryer: 4-6h, Processing Moisture Content: ≤0.02%, Melt Temperature Optimum: 280°C, Min. melt temperature: 270°C, Max. melt temperature: 290°C, Max. screw tangential speed: 0.2m/s, Mold Temperature Optimum: 110°C, Min. mold temperature: 100°C, Max. mold temperature: 120°C, Hold pressure range: ≥80MPa, Hold pressure time: 4s/mm, Back pressure: As low as possible, Ejection temperature: 170°C