Zytel® SC310 NC010

Want to keep this datasheet? Save it now in your required format

Description

Zytel® SC310 NC010 is a lubricated polyamide 66 resin for injection molding. It has been developed for consideration into applications such as parts for the healthcare industry.SPECIAL CONTROL for HEALTHCARE APPLICATIONSThis product is manufactured according to Good Manufacturing Practice (GMP) principles and generally accepted in food contact applications in Europe and the USA when meeting applicable use conditions. This product is also tested against ISO 10993-5 and -11 and selected parts of USP Class VI. For details, individual compliance statements are available from your DuPont representative.

Equivalent Materials

This material data has been provided by Matmatch.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueComment

Density

23.0 °C

1.14 g/cm³

Show Material materials with Density of 1.14 g/cm³

ISO 1183

Water absorption

23.0 °C

8.5 %

Show Material materials with Water absorption of 8.5 %

Sim. to ISO 62 | 80mil

Mechanical

PropertyTemperatureValueComment

Elastic modulus

23.0 °C

3.1 GPa

Show Material materials with Elastic modulus of 3.1 GPa

ISO 527-1/-2

Elongation

23.0 °C

25 %

Show Material materials with Elongation of 25 %

ISO 527-1/-2

Elongation at yield

23.0 °C

4.5 %

Show Material materials with Elongation at yield of 4.5 %

ISO 527-1/-2

Flexural modulus

23.0 °C

2.8 GPa

Show Material materials with Flexural modulus of 2.8 GPa

ISO 178

Hardness, Rockwell M

23.0 °C

79 [-]

Show Material materials with Hardness, Rockwell M of 79 [-]

ISO 2039-2

Hardness, Rockwell R

23.0 °C

121 [-]

Show Material materials with Hardness, Rockwell R of 121 [-]

ISO 2039-2

Impact strength, Charpy notched

-6.0 °C

4.5 kJ/m²

Show Material materials with Impact strength, Charpy notched of 4.5 kJ/m²

ISO 179/1eA

23.0 °C

5.5 kJ/m²

Show Material materials with Impact strength, Charpy notched of 5.5 kJ/m²

ISO 179/1eA

Impact strength, Charpy unnotched

-6.0 °C

400 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 400 kJ/m²

No Break @ 23°C, ISO 179/1eU

Poisson's ratio

23.0 °C

0.37 [-]

Show Material materials with Poisson's ratio of 0.37 [-]

Yield strength

23.0 °C

82 MPa

Show Material materials with Yield strength of 82 MPa

ISO 527-1/-2

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

23.0 °C

1E-4 1/K

Show Material materials with Coefficient of thermal expansion of 1E-4 1/K

ISO 11359-1/-2

Coefficient of thermal expansion, transverse

23.0 °C

1.1E-4 1/K

Show Material materials with Coefficient of thermal expansion, transverse of 1.1E-4 1/K

ISO 11359-1/-2

Glass transition temperature

60 °C

Show Material materials with Glass transition temperature of 60 °C

ISO 11357-1/-2 | 18°F/min

Heat deflection temperature, 0.45 MPa

200 °C

Show Material materials with Heat deflection temperature, 0.45 MPa of 200 °C

ISO 75-1/-2

Heat deflection temperature, 1.80 MPa

70 °C

Show Material materials with Heat deflection temperature, 1.80 MPa of 70 °C

ISO 75-1/-2

Melting point

262 °C

Show Material materials with Melting point of 262 °C

ISO 11357-1/-3 | 18°F/min

Specific heat capacity

23.0 °C

2790 J/(kg·K)

Show Material materials with Specific heat capacity of 2790 J/(kg·K)

of melt

Thermal diffusivity

23.0 °C

0 mm²/s

Show Material materials with Thermal diffusivity of 0 mm²/s

Vicat softening temperature

240 °C

Show Material materials with Vicat softening temperature of 240 °C

ISO 306 | 90°F/h, 11 lbf

Flammability

Burning Behav. at 60mil nom. thickn.: V-2 class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: V-2 class, Thickness tested: 0.7 mm, Oxygen index: 28 %

Electrical

PropertyTemperatureValueComment

Comparative tracking index

23.0 °C

600 V

Show Material materials with Comparative tracking index of 600 V

IEC 60112

Dielectric constant, 100Hz

23.0 °C

3.8 [-]

Show Material materials with Dielectric constant, 100Hz of 3.8 [-]

IEC 62631-2-1

Dielectric constant, 1MHz

23.0 °C

3.5 [-]

Show Material materials with Dielectric constant, 1MHz of 3.5 [-]

IEC 62631-2-1

Dielectric strength

23.0 °C

32 kV/mm

Show Material materials with Dielectric strength of 32 kV/mm

IEC 60243-1

Dissipation factor, 100Hz

23.0 °C

8E-3 [-]

Show Material materials with Dissipation factor, 100Hz of 8E-3 [-]

IEC 62631-2-1

Dissipation factor, 1MHz

23.0 °C

0.02 [-]

Show Material materials with Dissipation factor, 1MHz of 0.02 [-]

IEC 62631-2-1

Volume resistivity

23.0 °C

1.00E+14 Ω·cm

Show Material materials with Volume resistivity of 1.00E+14 Ω·cm

IEC 62631-3-1

Rheological Properties

PropertyTemperatureValueComment

Shrinkage

23.0 °C

1.4 %

Show Material materials with Shrinkage of 1.4 %

ISO 294-4, 2577

Shrinkage, transverse

23.0 °C

1.4 %

Show Material materials with Shrinkage, transverse of 1.4 %

ISO 294-4, 2577

Technological properties

Property
Processing methods

Drying Recommended: yes, Drying Temperature: 80°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.2%, Melt Temperature Optimum: 290°C, Min. melt temperature: 280°C, Max. melt temperature: 300°C, Max. screw tangential speed: 0.4m/s, Mold Temperature Optimum: 70°C, Min. mold temperature: 50°C, Max. mold temperature: 90°C, Hold pressure range: 50-100MPa, Hold pressure time: 4s/mm, Ejection temperature: 190°C