General
Property | Value |
---|---|
Density | 1.2 - 1.3 g/cm³ Show Material materials with Density of 1.2 - 1.3 g/cm³ |
Mechanical
Property | Value | Comment |
---|---|---|
Elastic modulus | 1.0 - 2.0 GPa Show Material materials with Elastic modulus of 1.0 - 2.0 GPa | |
Elongation | 2.0 - 15.0 % Show Material materials with Elongation of 2.0 - 15.0 % | |
Impact strength, Charpy notched | 2.0 - 5.0 kJ/m² Show Material materials with Impact strength, Charpy notched of 2.0 - 5.0 kJ/m² | |
Impact strength, Charpy unnotched | 21 kJ/m² Show Material materials with Impact strength, Charpy unnotched of 21 kJ/m² | |
Tensile strength | 18.0 - 38.0 MPa Show Material materials with Tensile strength of 18.0 - 38.0 MPa | at 2-15% strain |
Thermal
Property | Value |
---|---|
Melting point | 168.0 - 173.0 °C Show Material materials with Melting point of 168.0 - 173.0 °C |
Specific heat capacity | 1280.0 - 1290.0 J/(kg·K) Show Material materials with Specific heat capacity of 1280.0 - 1290.0 J/(kg·K) |
Flammability | UL 94 HB |
Electrical
Property | Value |
---|---|
Dielectric constant | 3 [-] Show Material materials with Dielectric constant of 3 [-] |
Electrical resistivity | 100000000000000 Ω·m Show Material materials with Electrical resistivity of 100000000000000 Ω·m |
Optical
Property | Value |
---|---|
Transparency | no |
Technological properties
Property | ||
---|---|---|
Application areas | Food packaging | |
Processing methods | Injection molding, extrusion, thermoforming |