Polycarbonate Reinforced with 20% Glass Fibre (PC+GF20)

Alternative and trade names
Makrolon®, Lupilon®, Edgetek™
Want to keep this datasheet? Save it now in your required format

Description

Reinforced Polycarbonate with 20% glass fiber with high viscosity and easy release.

This material data has been provided by M-Base.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValue

Density

1.3 - 1.35 g/cm³

Show Material materials with Density of 1.3 - 1.35 g/cm³

Mechanical

PropertyValueComment

Elastic modulus

5.6 - 6.5 GPa

Show Material materials with Elastic modulus of 5.6 - 6.5 GPa

Elongation

2.0 - 4.0 %

Show Material materials with Elongation of 2.0 - 4.0 %

Impact strength, Charpy notched

6.0 - 13.0 kJ/m²

Show Material materials with Impact strength, Charpy notched of 6.0 - 13.0 kJ/m²

Impact strength, Charpy unnotched

35 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 35 kJ/m²

60 kJ/m²

Show Material materials with Impact strength, Charpy unnotched of 60 kJ/m²

Tensile strength

50.0 - 110.0 MPa

Show Material materials with Tensile strength of 50.0 - 110.0 MPa

at 2-4% strain

Thermal

PropertyValue

Coefficient of thermal expansion

2.5e-05 - 7e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.5e-05 - 7e-05 1/K

Thermal conductivity

0.23 - 0.34 W/(m·K)

Show Material materials with Thermal conductivity of 0.23 - 0.34 W/(m·K)

Flammability

UL 94 V2-V0

Electrical

PropertyValue

Dielectric constant

3.2 [-]

Show Material materials with Dielectric constant of 3.2 [-]

3.4 [-]

Show Material materials with Dielectric constant of 3.4 [-]

Electrical resistivity

10000000000000.0 - 100000000000000.0 Ω·m

Show Material materials with Electrical resistivity of 10000000000000.0 - 100000000000000.0 Ω·m

Optical

PropertyValue

Transparency

no

Technological properties

Property
Application areas

housing parts, handheld surgical devices, electrical components, electrical boxes

Fillers

20% Glass Fiber

Processing methods

Injection molding, extrusion