General
Property | Value | Temperature |
---|---|---|
Density | 7.65 g/cm³ Show Material materials with Density of 7.65 g/cm³ at 23.0 °C | 23.0 °C |
Grain structure | Grain oriented electrical steel |
Dimension
Property | Value |
---|---|
Thickness | 0.27 mm Show Material materials with Thickness of 0.27 mm |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Elongation A80 | 6 - 14 % Show Material materials with Elongation A80 of 6 - 14 % at 23.0 °C | 23.0 °C | |
Elongation A80, transverse | 24 - 48 % Show Material materials with Elongation A80, transverse of 24 - 48 % at 23.0 °C | 23.0 °C | |
Hardness, Rockwell B | 75 - 85 [-] Show Material materials with Hardness, Rockwell B of 75 - 85 [-] at 23.0 °C | 23.0 °C | 15T |
Hardness, Vickers, 0.1 | 175 - 195 [-] Show Material materials with Hardness, Vickers, 0.1 of 175 - 195 [-] at 23.0 °C | 23.0 °C | |
Tensile strength | 330 - 370 MPa Show Material materials with Tensile strength of 330 - 370 MPa at 23.0 °C | 23.0 °C | |
Tensile strength, transverse | 390 - 420 MPa Show Material materials with Tensile strength, transverse of 390 - 420 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2 | 300 - 340 MPa Show Material materials with Yield strength Rp0.2 of 300 - 340 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2, transverse | 330 - 360 MPa Show Material materials with Yield strength Rp0.2, transverse of 330 - 360 MPa at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Comment |
---|---|---|
Max service temperature | 840 °C Show Material materials with Max service temperature of 840 °C | according to DIN IEC 60404-12, under inert gas for 2 h |
Electrical
Property | Value | Temperature | Comment |
---|---|---|---|
Electrical resistivity | 4.8E-7 Ω·m Show Material materials with Electrical resistivity of 4.8E-7 Ω·m at 23.0 °C | 23.0 °C | |
Surface insulation resistance | 10 Ω·cm² Show Material materials with Surface insulation resistance of 10 Ω·cm² at 23.0 °C | 23.0 °C | according to DIN IEC 60404-11 |
Magnetic
Property | Value | Temperature | Comment |
---|---|---|---|
Coercive force | 5 A/m Show Material materials with Coercive force of 5 A/m at 23.0 °C | 23.0 °C | |
Curie temperature | 745 °C Show Material materials with Curie temperature of 745 °C | ||
Guaranteed core loss | 0.9 [-] Show Material materials with Guaranteed core loss of 0.9 [-] at 23.0 °C | 23.0 °C | at 1.7 T and 50 Hz |
Guaranteed polarization | 1.88 [-] Show Material materials with Guaranteed polarization of 1.88 [-] at 23.0 °C | 23.0 °C | at 800 A/m |
Saturation polarization | 2.03 T Show Material materials with Saturation polarization of 2.03 T at 23.0 °C | 23.0 °C | |
Typical core loss | 0.88 [-] Show Material materials with Typical core loss of 0.88 [-] at 23.0 °C | 23.0 °C | at 1.7 T and 50 Hz |
Typical polarization | 1.91 [-] Show Material materials with Typical polarization of 1.91 [-] at 23.0 °C | 23.0 °C | at 800 A/m |
Technological properties
Property | ||
---|---|---|
Application areas | Large power transformers, distribution transformers, small transformers, current transformers, shunt reactors, wound cores, power generators | |
Coating | Both sides coated, coating thickness: 2 µm - 5 µm | |
Other | Advantages of powercore®: Energy efficiency thanks to minimal losses at full load and reduced no-load losses, reduced noise emission thanks to minimized magnetostriction and improved insulation properties, cost benefits thanks to lower core weights and more compact dimensions. |