SAE J775 Grade XEV-A

Want to keep this datasheet? Save it now in your required format

Related Standards

This material data has been provided by SAE.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

Properties

Mechanical

PropertyTemperatureValue

Reduction of area

20.0 °C

16 %

Show Material materials with Reduction of area of 16 %

650.0 °C

27 %

Show Material materials with Reduction of area of 27 %

760.0 °C

23 %

Show Material materials with Reduction of area of 23 %

Tensile strength

20.0 °C

1070 MPa

Show Material materials with Tensile strength of 1070 MPa

650.0 °C

640 MPa

Show Material materials with Tensile strength of 640 MPa

760.0 °C

510 MPa

Show Material materials with Tensile strength of 510 MPa

Unlock all property charts

Yield strength

20.0 °C

700 MPa

Show Material materials with Yield strength of 700 MPa

650.0 °C

330 MPa

Show Material materials with Yield strength of 330 MPa

760.0 °C

300 MPa

Show Material materials with Yield strength of 300 MPa

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.5 %

Show Material materials with Carbon of 0.5 %

Chromium

20.5 %

Show Material materials with Chromium of 20.5 %

Iron

63.5 - 100 %

Show Material materials with Iron of 63.5 - 100 %

Manganese

11.5 %

Show Material materials with Manganese of 11.5 %

Niobium

1 %

Show Material materials with Niobium of 1 %

Nitrogen

0.45 %

Show Material materials with Nitrogen of 0.45 %

Silicon

0.15 %

Show Material materials with Silicon of 0.15 %

Tungsten

2 %

Show Material materials with Tungsten of 2 %

Vanadium

0.4 %

Show Material materials with Vanadium of 0.4 %