DIN 17440 Grade X10Cr13 quenched and tempered (+QT)

Want to keep this datasheet? Save it now in your required format

Description

Application: - normally in quenched and tempered state with fine grounded or polished surface (tap elements, valve spindle, arbor, pump elements, bolts, screws) - application temperature: up to 550 °C - for construction elements in water and steam an mild acting media in food inustry

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 - 7.73 g/cm³

Show Material materials with Density of 7.7 - 7.73 g/cm³

Mechanical

PropertyTemperatureValue

Elastic modulus

20.0 °C

216 - 217.99 GPa

Show Material materials with Elastic modulus of 216 - 217.99 GPa

100.0 °C

213 - 215 GPa

Show Material materials with Elastic modulus of 213 - 215 GPa

200.0 °C

188 - 207 GPa

Show Material materials with Elastic modulus of 188 - 207 GPa

300.0 °C

164 - 200 GPa

Show Material materials with Elastic modulus of 164 - 200 GPa

400.0 °C

188.79 - 192 GPa

Show Material materials with Elastic modulus of 188.79 - 192 GPa

Elongation

20.0 °C

15 - 18 %

Show Material materials with Elongation of 15 - 18 %

Elongation, transverse

20.0 °C

12 %

Show Material materials with Elongation, transverse of 12 %

Poisson's ratio

20.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

100.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

200.0 °C

0.29 [-]

Show Material materials with Poisson's ratio of 0.29 [-]

300.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

400.0 °C

0.31 [-]

Show Material materials with Poisson's ratio of 0.31 [-]

Unlock all property charts

Shear modulus

20.0 °C

84.82 GPa

Show Material materials with Shear modulus of 84.82 GPa

100.0 °C

82.5 GPa

Show Material materials with Shear modulus of 82.5 GPa

200.0 °C

79.57 GPa

Show Material materials with Shear modulus of 79.57 GPa

300.0 °C

75.86 GPa

Show Material materials with Shear modulus of 75.86 GPa

400.0 °C

72 GPa

Show Material materials with Shear modulus of 72 GPa

Unlock all property charts

Tensile strength

20.0 °C

600 - 800 MPa

Show Material materials with Tensile strength of 600 - 800 MPa

Tensile strength, transverse

20.0 °C

600 - 800 MPa

Show Material materials with Tensile strength, transverse of 600 - 800 MPa

Yield strength Rp0.2

20.0 °C

420 MPa

Show Material materials with Yield strength Rp0.2 of 420 MPa

50.0 °C

430 MPa

Show Material materials with Yield strength Rp0.2 of 430 MPa

100.0 °C

420 MPa

Show Material materials with Yield strength Rp0.2 of 420 MPa

150.0 °C

410 MPa

Show Material materials with Yield strength Rp0.2 of 410 MPa

200.0 °C

400 MPa

Show Material materials with Yield strength Rp0.2 of 400 MPa

250.0 °C

382 MPa

Show Material materials with Yield strength Rp0.2 of 382 MPa

300.0 °C

365 MPa

Show Material materials with Yield strength Rp0.2 of 365 MPa

350.0 °C

335 MPa

Show Material materials with Yield strength Rp0.2 of 335 MPa

400.0 °C

305 MPa

Show Material materials with Yield strength Rp0.2 of 305 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

420 MPa

Show Material materials with Yield strength Rp0.2, transverse of 420 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

1.02E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.02E-5 1/K

100.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

200.0 °C

1.09E-5 - 1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.09E-5 - 1.1E-5 1/K

300.0 °C

1.13E-5 - 1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.13E-5 - 1.15E-5 1/K

400.0 °C

1.16E-5 - 1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.16E-5 - 1.2E-5 1/K

500.0 °C

1.2E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.2E-5 1/K

600.0 °C

1.22E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.22E-5 1/K

Unlock all property charts

Max service temperature, long

0 - 550 °C

Show Material materials with Max service temperature, long of 0 - 550 °C

Melting point

1370 - 1530 °C

Show Material materials with Melting point of 1370 - 1530 °C

Typical for Martensitic Stainless Steel

Specific heat capacity

20.0 °C

439 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 439 - 460 J/(kg·K)

100.0 °C

474 J/(kg·K)

Show Material materials with Specific heat capacity of 474 J/(kg·K)

200.0 °C

498 J/(kg·K)

Show Material materials with Specific heat capacity of 498 J/(kg·K)

300.0 °C

517 J/(kg·K)

Show Material materials with Specific heat capacity of 517 J/(kg·K)

400.0 °C

538 J/(kg·K)

Show Material materials with Specific heat capacity of 538 J/(kg·K)

500.0 °C

564 J/(kg·K)

Show Material materials with Specific heat capacity of 564 J/(kg·K)

600.0 °C

598 J/(kg·K)

Show Material materials with Specific heat capacity of 598 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

25.9 - 30 W/(m·K)

Show Material materials with Thermal conductivity of 25.9 - 30 W/(m·K)

100.0 °C

25.3 W/(m·K)

Show Material materials with Thermal conductivity of 25.3 W/(m·K)

200.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

300.0 °C

25.2 W/(m·K)

Show Material materials with Thermal conductivity of 25.2 W/(m·K)

400.0 °C

25.4 W/(m·K)

Show Material materials with Thermal conductivity of 25.4 W/(m·K)

500.0 °C

25.7 W/(m·K)

Show Material materials with Thermal conductivity of 25.7 W/(m·K)

600.0 °C

25.9 W/(m·K)

Show Material materials with Thermal conductivity of 25.9 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

7.6 mm²/s

Show Material materials with Thermal diffusivity of 7.6 mm²/s

100.0 °C

6.6 mm²/s

Show Material materials with Thermal diffusivity of 6.6 mm²/s

200.0 °C

6.1 mm²/s

Show Material materials with Thermal diffusivity of 6.1 mm²/s

300.0 °C

5.8 mm²/s

Show Material materials with Thermal diffusivity of 5.8 mm²/s

400.0 °C

5.3 mm²/s

Show Material materials with Thermal diffusivity of 5.3 mm²/s

500.0 °C

4.8 mm²/s

Show Material materials with Thermal diffusivity of 4.8 mm²/s

600.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

5.59E-7 - 6E-7 Ω·m

Show Material materials with Electrical resistivity of 5.59E-7 - 6E-7 Ω·m

100.0 °C

6.4E-7 Ω·m

Show Material materials with Electrical resistivity of 6.4E-7 Ω·m

200.0 °C

7.32E-7 Ω·m

Show Material materials with Electrical resistivity of 7.32E-7 Ω·m

300.0 °C

8.17E-7 Ω·m

Show Material materials with Electrical resistivity of 8.17E-7 Ω·m

400.0 °C

8.97E-7 Ω·m

Show Material materials with Electrical resistivity of 8.97E-7 Ω·m

500.0 °C

9.74E-7 Ω·m

Show Material materials with Electrical resistivity of 9.74E-7 Ω·m

600.0 °C

1.05E-6 Ω·m

Show Material materials with Electrical resistivity of 1.05E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.08 - 0.12 %

Show Material materials with Carbon of 0.08 - 0.12 %

Chromium

12 - 14 %

Show Material materials with Chromium of 12 - 14 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Phosphorus

0.05 %

Show Material materials with Phosphorus of 0.05 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.03 %

Show Material materials with Sulfur of 0.03 %