EN 10088-1 Grade X3CrTi17 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

Acc. VdTÜV material data sheet 494 : 1996-06 the stainless ferritic steel X 6 CrTi 17, mat. no. 1.4510, is used for longitudinal welded tubes for pressure vessels acc. TRB 100 and AD data sheet W 2 at operating temperatures from - 10 to 280 °C. and pressures up to 50 bar and for type approved hot water boiler up to 100 °C. The weldability is examined allowing for the generally accepted engineering rules for inert arc welding without filler or with wire electrode and for seam welding. Preheating is mostly not necessary, the intermediate layer temperature amounts to max. 200 °C. An heat treatment after the welding is unusual. Longitudinal welded tubes have to recrystallising annealed. The material is also in the welded condition resistant against intercrystalline corrosion. For the material acc. DIN EN 10088-1 : 1995-08 applies: The mark X3CrTi17 is comparable to X 6 CrTi 17 (here higher C-content). This material is a ferritic steel with comparable general corrosion properties like 1.4016. It is widely resistant in water, steam, weak acids and bases as well as in oxidizing acids. The steel shows increased stress corrosion resistance in hot bases, low chloride containing water. No risk of intercrystalline corrosion after welding due to Ti-addition, but it is therefore unsuitable for mirror finishing. Application for welded parts in washing machines (lye tanks) and partly in chemical apparatus engineering (weak acids), in dairy, food, brewery, dyeing and soap industry.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.56 - 7.7 g/cm³

Show Material materials with Density of 7.56 - 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

218 - 220 GPa

Show Material materials with Elastic modulus of 218 - 220 GPa

100.0 °C

213 - 215 GPa

Show Material materials with Elastic modulus of 213 - 215 GPa

200.0 °C

206 - 210 GPa

Show Material materials with Elastic modulus of 206 - 210 GPa

300.0 °C

198 - 205 GPa

Show Material materials with Elastic modulus of 198 - 205 GPa

400.0 °C

190 - 195 GPa

Show Material materials with Elastic modulus of 190 - 195 GPa

500.0 °C

180 GPa

Show Material materials with Elastic modulus of 180 GPa

600.0 °C

167 GPa

Show Material materials with Elastic modulus of 167 GPa

700.0 °C

150 GPa

Show Material materials with Elastic modulus of 150 GPa

Elongation

20.0 °C

23 %

Show Material materials with Elongation of 23 %

Elongation A80

20.0 °C

23 %

Show Material materials with Elongation A80 of 23 %

Elongation A80, transverse

20.0 °C

23 %

Show Material materials with Elongation A80, transverse of 23 %

Elongation, transverse

20.0 °C

23 %

Show Material materials with Elongation, transverse of 23 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Ferritic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Ferritic Stainless Steel

Tensile strength

20.0 °C

420 - 600 MPa

Show Material materials with Tensile strength of 420 - 600 MPa

Tensile strength, transverse

20.0 °C

420 - 600 MPa

Show Material materials with Tensile strength, transverse of 420 - 600 MPa

Yield strength Rp0.2

20.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

100.0 °C

195 MPa

Show Material materials with Yield strength Rp0.2 of 195 MPa

150.0 °C

190 MPa

Show Material materials with Yield strength Rp0.2 of 190 MPa

200.0 °C

185 MPa

Show Material materials with Yield strength Rp0.2 of 185 MPa

250.0 °C

175 MPa

Show Material materials with Yield strength Rp0.2 of 175 MPa

300.0 °C

165 MPa

Show Material materials with Yield strength Rp0.2 of 165 MPa

350.0 °C

155 MPa

Show Material materials with Yield strength Rp0.2 of 155 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

240 MPa

Show Material materials with Yield strength Rp0.2, transverse of 240 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

20.0 °C

9.9E-6 1/K

Show Material materials with Coefficient of thermal expansion of 9.9E-6 1/K

100.0 °C

1E-5 - 1.03E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 - 1.03E-5 1/K

200.0 °C

1E-5 - 1.08E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 - 1.08E-5 1/K

300.0 °C

1.05E-5 - 1.12E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.12E-5 1/K

400.0 °C

1.05E-5 - 1.16E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 - 1.16E-5 1/K

500.0 °C

1.1E-5 - 1.19E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 - 1.19E-5 1/K

600.0 °C

1.21E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.21E-5 1/K

700.0 °C

1.24E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.24E-5 1/K

800.0 °C

1.29E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.29E-5 1/K

Unlock all property charts

Max service temperature, long

-10 - 280 °C

Show Material materials with Max service temperature, long of -10 - 280 °C

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

450 - 460 J/(kg·K)

Show Material materials with Specific heat capacity of 450 - 460 J/(kg·K)

100.0 °C

482 J/(kg·K)

Show Material materials with Specific heat capacity of 482 J/(kg·K)

200.0 °C

506 J/(kg·K)

Show Material materials with Specific heat capacity of 506 J/(kg·K)

300.0 °C

525 J/(kg·K)

Show Material materials with Specific heat capacity of 525 J/(kg·K)

400.0 °C

547 J/(kg·K)

Show Material materials with Specific heat capacity of 547 J/(kg·K)

500.0 °C

576 J/(kg·K)

Show Material materials with Specific heat capacity of 576 J/(kg·K)

600.0 °C

616 J/(kg·K)

Show Material materials with Specific heat capacity of 616 J/(kg·K)

Unlock all property charts

Thermal conductivity

20.0 °C

16 - 25 W/(m·K)

Show Material materials with Thermal conductivity of 16 - 25 W/(m·K)

100.0 °C

17.2 W/(m·K)

Show Material materials with Thermal conductivity of 17.2 W/(m·K)

200.0 °C

18.6 W/(m·K)

Show Material materials with Thermal conductivity of 18.6 W/(m·K)

300.0 °C

20 W/(m·K)

Show Material materials with Thermal conductivity of 20 W/(m·K)

400.0 °C

21.2 W/(m·K)

Show Material materials with Thermal conductivity of 21.2 W/(m·K)

500.0 °C

22.3 W/(m·K)

Show Material materials with Thermal conductivity of 22.3 W/(m·K)

600.0 °C

23.3 W/(m·K)

Show Material materials with Thermal conductivity of 23.3 W/(m·K)

700.0 °C

24.1 W/(m·K)

Show Material materials with Thermal conductivity of 24.1 W/(m·K)

800.0 °C

25.5 W/(m·K)

Show Material materials with Thermal conductivity of 25.5 W/(m·K)

900.0 °C

26.9 W/(m·K)

Show Material materials with Thermal conductivity of 26.9 W/(m·K)

1000.0 °C

28.3 W/(m·K)

Show Material materials with Thermal conductivity of 28.3 W/(m·K)

Unlock all property charts

Thermal diffusivity

20.0 °C

4.7 mm²/s

Show Material materials with Thermal diffusivity of 4.7 mm²/s

100.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

200.0 °C

4.5 mm²/s

Show Material materials with Thermal diffusivity of 4.5 mm²/s

300.0 °C

4.6 mm²/s

Show Material materials with Thermal diffusivity of 4.6 mm²/s

400.0 °C

4.4 mm²/s

Show Material materials with Thermal diffusivity of 4.4 mm²/s

500.0 °C

4.1 mm²/s

Show Material materials with Thermal diffusivity of 4.1 mm²/s

600.0 °C

3.6 mm²/s

Show Material materials with Thermal diffusivity of 3.6 mm²/s

Unlock all property charts

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6E-7 - 9.06E-7 Ω·m

Show Material materials with Electrical resistivity of 6E-7 - 9.06E-7 Ω·m

100.0 °C

9.42E-7 Ω·m

Show Material materials with Electrical resistivity of 9.42E-7 Ω·m

200.0 °C

9.87E-7 Ω·m

Show Material materials with Electrical resistivity of 9.87E-7 Ω·m

300.0 °C

1.03E-6 Ω·m

Show Material materials with Electrical resistivity of 1.03E-6 Ω·m

400.0 °C

1.08E-6 Ω·m

Show Material materials with Electrical resistivity of 1.08E-6 Ω·m

500.0 °C

1.12E-6 Ω·m

Show Material materials with Electrical resistivity of 1.12E-6 Ω·m

600.0 °C

1.18E-6 Ω·m

Show Material materials with Electrical resistivity of 1.18E-6 Ω·m

700.0 °C

1.22E-6 Ω·m

Show Material materials with Electrical resistivity of 1.22E-6 Ω·m

800.0 °C

1.24E-6 Ω·m

Show Material materials with Electrical resistivity of 1.24E-6 Ω·m

900.0 °C

1.26E-6 Ω·m

Show Material materials with Electrical resistivity of 1.26E-6 Ω·m

1000.0 °C

1.27E-6 Ω·m

Show Material materials with Electrical resistivity of 1.27E-6 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Carbon

0.05 %

Show Material materials with Carbon of 0.05 %

Chromium

16 - 18 %

Show Material materials with Chromium of 16 - 18 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Titanium

0.8 %