EN 10088-1 Grade X2CrMoTi17-1 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

The ferritic steel X2CrMoTi17-1 (special grade, annealed) is well formable. It is used for household appliances and pipes.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 g/cm³

Show Material materials with Density of 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

220 GPa

Show Material materials with Elastic modulus of 220 GPa

100.0 °C

215 GPa

Show Material materials with Elastic modulus of 215 GPa

200.0 °C

210 GPa

Show Material materials with Elastic modulus of 210 GPa

300.0 °C

205 GPa

Show Material materials with Elastic modulus of 205 GPa

400.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

Elongation

20.0 °C

23 %

Show Material materials with Elongation of 23 %

Elongation A80

20.0 °C

23 %

Show Material materials with Elongation A80 of 23 %

Elongation A80, transverse

20.0 °C

23 %

Show Material materials with Elongation A80, transverse of 23 %

Elongation, transverse

20.0 °C

23 %

Show Material materials with Elongation, transverse of 23 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Ferritic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Ferritic Stainless Steel

Tensile strength

20.0 °C

400 - 550 MPa

Show Material materials with Tensile strength of 400 - 550 MPa

Tensile strength, transverse

20.0 °C

400 - 550 MPa

Show Material materials with Tensile strength, transverse of 400 - 550 MPa

Yield strength Rp0.2

20.0 °C

200 MPa

Show Material materials with Yield strength Rp0.2 of 200 MPa

Yield strength Rp0.2, transverse

20.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2, transverse of 220 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1E-5 1/K

200.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

300.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

400.0 °C

1.05E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.05E-5 1/K

500.0 °C

1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K

Unlock all property charts

Melting point

1425 - 1530 °C

Show Material materials with Melting point of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Specific heat capacity

20.0 °C

460 J/(kg·K)

Show Material materials with Specific heat capacity of 460 J/(kg·K)

Thermal conductivity

20.0 °C

25 W/(m·K)

Show Material materials with Thermal conductivity of 25 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

7E-7 Ω·m

Show Material materials with Electrical resistivity of 7E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.025 %

Show Material materials with Carbon of 0.025 %

Chromium

16 - 18 %

Show Material materials with Chromium of 16 - 18 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Molybdenum

0.8 - 1.4 %

Show Material materials with Molybdenum of 0.8 - 1.4 %

Nitrogen

0.02 %

Show Material materials with Nitrogen of 0.02 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %

Titanium

0.3 - 0.6 %

Show Material materials with Titanium of 0.3 - 0.6 %