EN 10088-1 Grade X2CrNbZr17 soft annealed (+A)

Want to keep this datasheet? Save it now in your required format

Description

The zircon-alloyed patented steel X2CrNbZr17 is used as cold rolled strip. It shows resistance to intercrystalline corrosion both in delivery and welded condition. The material may be used as heat-resistant steel acc. to DIN EN 10095 : 1999-05.

Related Standards

Equivalent Materials

This material data has been provided by WIAM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValue

Density

20.0 °C

7.7 g/cm³

Show Material materials with Density of 7.7 g/cm³

Mechanical

PropertyTemperatureValueComment

Elastic modulus

20.0 °C

220 GPa

Show Material materials with Elastic modulus of 220 GPa

100.0 °C

215 GPa

Show Material materials with Elastic modulus of 215 GPa

200.0 °C

210 GPa

Show Material materials with Elastic modulus of 210 GPa

300.0 °C

205 GPa

Show Material materials with Elastic modulus of 205 GPa

400.0 °C

195 GPa

Show Material materials with Elastic modulus of 195 GPa

Elongation

20.0 °C

23 %

Show Material materials with Elongation of 23 %

Elongation A80

20.0 °C

23 %

Show Material materials with Elongation A80 of 23 %

Elongation A80, transverse

20.0 °C

23 %

Show Material materials with Elongation A80, transverse of 23 %

Elongation, transverse

20.0 °C

23 %

Show Material materials with Elongation, transverse of 23 %

Poisson's ratio

23.0 °C

0.3 [-]

Show Material materials with Poisson's ratio of 0.3 [-]

Typical for Austenitic Stainless Steel

Shear modulus

23.0 °C

77 GPa

Show Material materials with Shear modulus of 77 GPa

Typical for Austenitic Stainless Steel

Tensile strength

20.0 °C

400 - 550 MPa

Show Material materials with Tensile strength of 400 - 550 MPa

Tensile strength, transverse

20.0 °C

400 - 550 MPa

Show Material materials with Tensile strength, transverse of 400 - 550 MPa

Yield strength Rp0.2

20.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

100.0 °C

230 MPa

Show Material materials with Yield strength Rp0.2 of 230 MPa

150.0 °C

220 MPa

Show Material materials with Yield strength Rp0.2 of 220 MPa

200.0 °C

210 MPa

Show Material materials with Yield strength Rp0.2 of 210 MPa

250.0 °C

205 MPa

Show Material materials with Yield strength Rp0.2 of 205 MPa

300.0 °C

200 MPa

Show Material materials with Yield strength Rp0.2 of 200 MPa

350.0 °C

180 MPa

Show Material materials with Yield strength Rp0.2 of 180 MPa

Unlock all property charts

Yield strength Rp0.2, transverse

20.0 °C

250 MPa

Show Material materials with Yield strength Rp0.2, transverse of 250 MPa

Thermal

PropertyTemperatureValueComment

Coefficient of thermal expansion

100.0 °C

1.1E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.1E-5 1/K

300.0 °C

1.15E-5 1/K

Show Material materials with Coefficient of thermal expansion of 1.15E-5 1/K

Unlock all property charts

Melting point

1230 - 1480 °C

Show Material materials with Melting point of 1230 - 1480 °C

Typical for Austenitic Stainless Steel

Specific heat capacity

20.0 °C

460 J/(kg·K)

Show Material materials with Specific heat capacity of 460 J/(kg·K)

Thermal conductivity

20.0 °C

26 W/(m·K)

Show Material materials with Thermal conductivity of 26 W/(m·K)

Electrical

PropertyTemperatureValue

Electrical resistivity

20.0 °C

6E-7 Ω·m

Show Material materials with Electrical resistivity of 6E-7 Ω·m

Chemical properties

PropertyValue

Carbon

0.03 %

Show Material materials with Carbon of 0.03 %

Chromium

16 - 17.5 %

Show Material materials with Chromium of 16 - 17.5 %

Manganese

1 %

Show Material materials with Manganese of 1 %

Niobium

0.35 - 0.55 %

Show Material materials with Niobium of 0.35 - 0.55 %

Phosphorus

0.04 %

Show Material materials with Phosphorus of 0.04 %

Silicon

1 %

Show Material materials with Silicon of 1 %

Sulfur

0.015 %

Show Material materials with Sulfur of 0.015 %